Where it is used
Stiff, dimensionally stable enclosure and tooling parts; Bambu Lab notes the fibre blurs layer lines into a matte finish
Sources
- Bambu Filament Technical Data Sheet V1.0 — ABS-GF · 2026-08 · tds
ABS with chopped glass fibre: HDT rises to 99 °C at 0.45 MPa and layer lines blur into a matte finish, while notched Charpy collapses from 21.5 to 4.2 kJ/m².
Open in interactive comparisonStiff, dimensionally stable enclosure and tooling parts; Bambu Lab notes the fibre blurs layer lines into a matte finish
ABS with chopped glass fibre: HDT rises to 99 °C at 0.45 MPa and layer lines blur into a matte finish, while notched Charpy collapses from 21.5 to 4.2 kJ/m².
ABS-GF is suited to rigid housings, tooling and dimensionally stable mechanical components. Glass reinforcement raises modulus and can reduce the warping associated with unfilled ABS. 3DXTech positions FibreX ABS+GF for structural engineering applications, while Bambu’s documented grade also offers a matte surface that visually softens layer lines.
Glass-filled ABS is not interchangeable with tough unfilled ABS. In Bambu’s grade comparison, notched impact resistance falls substantially even as stiffness and heat deflection improve. That favors rigid screwed or supported geometry over thin spring clips and impact-prone tabs. Fiber content and matrix formulation vary between products, and the abrasive reinforcement requires suitable printing hardware.
FDM · 3DXTech FibreX ABS+GF · Manufacturer-listed applications
3DXTech lists structural engineering uses for FibreX ABS+GF and emphasizes stiffness and reduced printing distortion. This identifies the intended function of that glass-filled grade, not a production case study or universal impact-performance claim.
Check the model’s material and process notes before choosing a filament.
Representative catalog values. Check the exact grade and its linked conditions before using a setting.
240–280 (Bambu Lab)
240–280 (Bambu Lab)
80–100 (Bambu Lab)
80–100 (Bambu Lab)
Enclosure recommended
Enclosure recommended — Bambu Lab specifies a 45–60 °C chamber
80 °C for 8 h (Bambu Lab)
80 °C for 8 h (Bambu Lab)
Open a topic to explore the complete data. Each value keeps its original conditions, units and dated sources.
| Property and unit | Published value and conditions | Sources and dates |
|---|---|---|
| Base polymer / chemistry | ABS reinforced with chopped glass fibre — 3DXTech's grade is nominally 10 wt% | 2 sources
|
| Density (g/cm³) | 1.08 (Bambu Lab) and 1.15 (3DXTech), ISO 1183 | 2 sources
|
| Typical price (USD/kg) | 1 kg-equivalent spools span 24–73; the middle of the market is about 35 | 4 sources
|
| Price range across brands (USD/kg) | 24–73 across brands; Siraya Tech 24, Bambu Lab 30, SUNLU 40, 3DXTech 73 | 4 sources
|
| Market availability (1–5) | Available from several mainstream brands | 2 sources
|
| Spool sizes & diameters | 1.75 and 2.85 mm; 750 g and 1 kg spools | 2 sources
|
| Typical applications | Stiff, dimensionally stable enclosure and tooling parts; Bambu Lab notes the fibre blurs layer lines into a matte finish | 1 source
|
| Property and unit | Published value and conditions | Sources and dates |
|---|---|---|
| Nozzle temperature (°C) | 240–280 (Bambu Lab) | 1 source
|
| Bed temperature (°C) | 80–100 (Bambu Lab) | 1 source
|
| Enclosure / chamber requirement (1–5) | Enclosure recommended — Bambu Lab specifies a 45–60 °C chamber | 2 sources
|
| Recommended chamber temperature (°C) | 45–60 (Bambu Lab) | 1 source
|
| Part cooling fan | 0–80 % (Bambu Lab) | 1 source
|
| Bed surface & adhesion aid | Clean the plate and apply glue; Simplify3D also lists Kapton tape and ABS slurry | 2 sources
|
| Maximum volumetric flow (mm³/s; see test conditions) (mm³/s) | 14 at Bambu Lab's 180 mm/s cap on a 0.4 mm nozzle at 0.2 mm layer | 2 sources
|
| Warping tendency (1–5) | Moderate — needs adhesion aid or draught shield; Bambu Lab positions the fibre as reducing warping | 1 source
|
| Bed-adhesion difficulty (1–5) | Needs a specific surface plus adhesive | 1 source
|
| Stringing / oozing tendency (1–5) | Slight — Polymaker advises 1–2 mm retraction at 20–30 mm/s | 1 source
|
| Overall printing difficulty (1–5) | Intermediate — dry filament and a tuned profile; hardened nozzle mandatory | 1 source
|
| Property and unit | Published value and conditions | Sources and dates |
|---|---|---|
| Nozzle hardness required (1–4) | Hardened steel required | 1 source
|
| Abrasiveness (1–5) | Highly abrasive — standard GF composite | 1 source
|
| Nozzle clog risk (1–5) | Moderate — needs dry filament and a clean nozzle; 3DXTech specifies a hardened 0.4 mm minimum nozzle and 0.25 mm layers or higher for the glass-filled grade | 2 sources
|
| Heat-creep / jam sensitivity (1–5) | Slightly sensitive | 1 source
|
| Hotend requirement | No special hot-end required | 1 source
|
| Property and unit | Published value and conditions | Sources and dates |
|---|---|---|
| Moisture absorption (hygroscopicity) (1–5) | Moderate — 0.53 % saturated at 25 °C / 55 % RH (Bambu Lab) | 1 source
|
| Equilibrium moisture content at ~50 % RH (%) | 0.53 saturated at 25 °C / 55 % RH (Bambu Lab) | 1 source
|
| Drying temperature & time | 80 °C for 8 h (Bambu Lab) | 1 source
|
| Symptoms when wet | Bubbling and popping at the nozzle, stringing and a rough surface | 1 source
|
| Effect of moisture on strength | Polymaker rates ABS moderate-sensitivity and publishes no dry-versus-conditioned figures; absorbed water flashes to steam in the hotend and shows as bubbling and poor layer adhesion | 1 source
|
| Storage requirement | Sealed with desiccant; Polymaker rates ABS moderate-sensitivity | 1 source
|
| Property and unit | Published value and conditions | Sources and dates |
|---|---|---|
| Tensile strength (XY) (MPa) | 36 ± 3 printed XY, ISO 527 (Bambu Lab); 3DXTech quotes 68 at break | 2 sources
|
| Young's modulus (MPa) | 3160 ± 170 printed XY, ISO 527 (Bambu Lab); 3DXTech quotes 4210 | 2 sources
|
| Elongation at break (%) | 6.3 ± 1.2 printed XY, ISO 527 (Bambu Lab); 3DXTech quotes 2 at break | 2 sources
|
| Flexural strength (MPa) | 68 ± 4 printed XY, ISO 178 (Bambu Lab); 3DXTech quotes 70 | 2 sources
|
| Flexural modulus (MPa) | 2860 ± 130 printed XY, ISO 178 (Bambu Lab); 3DXTech quotes 4420 | 2 sources
|
| Charpy impact, notched (kJ/m²) | 4.2 ± 1.1 printed XY, ISO 179, notched (Bambu Lab) | 1 source
|
| Other impact data | Charpy unnotched 14.5 ± 1.5 printed XY (Bambu Lab, ISO 179) | 1 source
|
| Layer adhesion / Z tensile (MPa) | 29 ± 3 printed Z, ISO 527 (Bambu Lab) | 1 source
|
| Brittleness (1–5) | Brittle — snaps with little warning; notched Charpy falls from 21.5 to 4.2 kJ/m² against unfilled Bambu Lab ABS | 2 sources
|
| Creep resistance / sustained load (1–5) | Good — no creep test found; chopped glass fibre lifts modulus to 3160 MPa against 2200 for unfilled Bambu Lab ABS | 2 sources
|
| Fatigue / repeated-flex resistance (1–5) | Below average — no S-N curve found; notched Charpy falls to 4.2 kJ/m² against 21.5 for unfilled Bambu Lab ABS | 2 sources
|
| Elasticity / flexibility (1–5) | Rigid | 1 source
|
| Z strength as % of XY (%) | 81 (Bambu Lab, printed Z against XY tensile) | 1 source
|
| Property and unit | Published value and conditions | Sources and dates |
|---|---|---|
| HDT at 0.45 MPa (°C) | 99 (ISO 75, 0.45 MPa, Bambu Lab) against 87 for unfilled Bambu Lab ABS | 2 sources
|
| HDT at 1.8 MPa (°C) | 88 (ISO 75, 1.8 MPa, Bambu Lab) against 84 for unfilled Bambu Lab ABS | 2 sources
|
| Property and unit | Published value and conditions | Sources and dates |
|---|---|---|
| Chemical resistance | Good against weak acids, weak alkalis, oils and grease; dissolved by acetone | 1 source
|
| Food contact | Not food safe — Polymaker cites potential chemical leaching | 1 source
|
| Biodegradability / compostability | Not biodegradable | 1 source
|
| Recyclability | Mechanically recyclable but not accepted in household plastic collection | 1 source
|
| Property and unit | Published value and conditions | Sources and dates |
|---|---|---|
| Fume toxicity (1–5) | High — hazardous VOC such as styrene; enclosure and filtration needed | |
| VOC emission rate (µg/min) | 12–113 styrene, the dominant VOC from every ABS and HIPS combination tested | |
| Ultrafine-particle emission rate (particles/min) | 2 × 10¹⁰ to 9 × 10¹⁰ median across all ABS printers, two orders of magnitude above PLA's ≈1 × 10⁸ | |
| Hazardous species emitted | Styrene dominates. Bambu Lab states ABS and ASA release harmful gases such as styrene at printing temperature, which can be toxic and cause dizziness or nausea | |
| Ventilation / filtration requirement (1–5) | Enclosure with carbon and HEPA filtration — an enclosure alone cut measured UFP by only about 35 % | |
| Dust & fibre handling hazard | Glass fibre is bound in the matrix; avoid inhaling sanding dust | 1 source
|
| Property and unit | Published value and conditions | Sources and dates |
|---|---|---|
| Sanding & machining | Sands well and takes filler before painting | 1 source
|
| Painting & finishing | Paints readily after light abrasion | 1 source
|
| Support material pairing | HIPS breaks away or dissolves in d-limonene; Bambu Lab sells a dedicated Support for ABS | 2 sources
|
| Dimensional accuracy & detail | Bambu Lab describes a smooth matte finish with micro-spot gloss that blurs layer lines | 1 source
|
| Property and unit | Published value and conditions | Sources and dates |
|---|---|---|
| Soluble in | Acetone dissolves the resin and leaves the fibre as sludge; MEK, THF, ethyl acetate and chlorinated solvents do the same. | 2 sources |
| Softened or crazed by | Petrol and perchloroethylene soften it and benzene attacks it; d-limonene disrupts layer adhesion in some ABS and ASA grades. | 2 sources
|
| Solvent welding & smoothing agent | Acetone vapour reaches only the resin fraction, so the fibre is left standing proud of the smoothed surface. | 2 sources
|
Values describe representative grades, not every spool. Manufacturer datasheets and independent tests retain their source labels and dates. Printed orientation, test method, conditioning and formulation can change results. Unknown values are —. A listed use is not a certification. Shore A, Shore D and Rockwell hardness are separate scales.
Historical USD/kg snapshots. Read each listing’s sale/from qualifiers, spool mass, source date, shipping and tax notes. Product figures are separate from the material summary.
$24.49 / 1 kg spool, siraya.tech US store, Aug 2026 (list $34.99)
10 % glass fibre. Hardened steel nozzle specified.
Open product listing ↗| Density (g/cm³) | 1.08 (ISO 1183) |
|
|---|---|---|
| Nozzle temperature (°C) | 250-270 |
|
| Bed temperature (°C) | 100-110 |
|
| Tensile strength (XY) (MPa) | 44 +/- 3 (printed XY, ISO 527) |
|
| Young's modulus (MPa) | 2350 (ASTM D638) |
|
| Elongation at break (%) | 3 (printed XY, ASTM D638) |
|
| Flexural strength (MPa) | 66.4 (flexural, standard not stated) |
|
| Flexural modulus (MPa) | 2705 (flexural, standard not stated) |
|
| Charpy impact, notched (kJ/m²) | 8.5 (Charpy, standard not stated) |
|
| Hardness (scale-specific) (Shore A / Shore D / Rockwell) | 82 Shore D |
|
| HDT at 0.45 MPa (°C) | 97 (method B, 0.45 MPa) |
|
| HDT at 1.8 MPa (°C) | 93 (method A, 1.8 MPa) |
|
| Glass transition (Tg) (°C) | 101 |
|
$29.99 / 1 kg spool, us.store.bambulab.com, Aug 2026
HDT rises to 99 °C at 0.45 MPa but notched Charpy falls to 4.2 kJ/m² from 21.5 for unfilled Bambu Lab ABS.
Open product listing ↗| Density (g/cm³) | 1.08 (ISO 1183) |
|
|---|---|---|
| Young's modulus (MPa) | 3160 ± 170 (printed XY, ISO 527) |
|
| Charpy impact, notched (kJ/m²) | 4.2 ± 1.1 (printed XY, ISO 179, notched) |
|
| HDT at 0.45 MPa (°C) | 99 (ISO 75, 0.45 MPa) |
|
Regular $39.99 / 1 kg spool, store.sunlu.com, Aug 2026; a 15 % back-to-school flash deal was showing $26.99
10 % glass fibre. Vendor compares 54 MPa tensile and 90 MPa flexural against its own unfilled ABS but names no test standard. SUNLU quotes flexural strength 90 MPa and tensile 54 MPa against 55 MPa and 42 MPa for its standard ABS, without naming a test standard or specimen type.
Open product listing ↗| Base polymer / chemistry | ABS filled with 10 % glass fibre |
|
|---|---|---|
| Spool sizes & diameters | 1 kg spool; 1.75 mm |
|
| Nozzle temperature (°C) | 260-280 |
|
| Bed temperature (°C) | 90-100 |
|
| Part cooling fan | Auxiliary fan off; part cooling fan 10 % or less |
|
| Bed surface & adhesion aid | Apply adhesive to the build plate |
|
$55.00 / 750 g spool = $73.33/kg, 3dxtech.com product catalogue, Aug 2026
Handle fibrex-abs-gf-1. Tensile strength at break 68 MPa, the highest here.
Open product listing ↗| Density (g/cm³) | 1.15 (ISO 1183) |
|
|---|---|---|
| Nozzle temperature (°C) | 245 (TDS printed-specimen condition) |
|
| Bed temperature (°C) | 110 (TDS printed-specimen condition) |
|
| Tensile strength (XY) (MPa) | 68 at break (ISO 527) |
|
| Young's modulus (MPa) | 4210 (ISO 527) |
|
| Elongation at break (%) | 2 at break (printed XY, ISO 527) |
|
| Flexural strength (MPa) | 70 (printed XY, ISO 178) |
|
| Flexural modulus (MPa) | 4420 (printed XY, ISO 178) |
|
| HDT at 0.45 MPa (°C) | 98 (ISO 75, 0.45 MPa) |
|
| Glass transition (Tg) (°C) | 105 (DSC) |
|
| Electrical & ESD properties | Surface resistance >10^13 Ω/sq (ASTM D257) |
|