Filament comparison
PLA Matte vs PPS-CF
Compare printing settings, strength, heat resistance, dated prices and sources.
2 selected · all documented properties
| Property | Matte PLAPLA | Fibre-reinforced PPSHIGHTEMP |
|---|---|---|
| Market snapshot | ||
| Listing priceUSD/kg; dated snapshots | $19.09/kg median; $10.99–$32.16/kg across 10 dated product listings | $139.98/kg median; $119.98–$174.17/kg across 5 dated product listings |
| Identity & Market | ||
| Base polymer / chemistry | PLA compounded with a mineral filler — Fiberlogy names chalk — that scatters light into a diffuse finish[1][2] | Carbon-fibre reinforced PPS — Polymaker's Fiberon grade is nominally 10 wt%[3] |
| Densityg/cm³ | 1.31 (Bambu Lab, ISO 1183) to 1.38 (Fiberlogy PLA Mineral, method not stated) — above plain PLA from the filler[2][1] | 1.29 (Fiberon PPS-CF10) and 1.36 (Fiberon PPS-GF20), ISO 1183[3][4] |
| Typical priceUSD/kg | Mainstream 1 kg spools cluster near 21[5][6][7] | 1 kg-equivalent spools span 93–174; the middle of the market is about 140[8][9][10][11] |
| Price range across brandsUSD/kg | 11–32 across brands; budget house brands 11–19, Fiberlogy PLA Mineral 32[12][6][13] | 93-174 across brands and formats; Polymaker Fiberon PPS-GF20 93 at 3 kg, IEMAI 3D CF-PPS 131 at 750 g, LEHVOSS Luvocom 3F PPS CF 9938 164 at 2.3 kg, Bambu Lab PPS-CF 174 at 750 g[8][9][10][11] |
| Market availability1–5 | Stocked by most mainstream brands[12][7][5] | Available from several mainstream brands[8][9][10] |
| Spool sizes & diameters | 1.75 mm; 1 kg spools plus spool-less refills[5][14] | 1.75 mm; 0.5 kg spools[8] |
| Typical applications | Display models and visible parts where a matte, non-reflective finish matters[2] | Chemical and automotive parts needing PPS chemistry with structural stiffness[3] |
| Diameter tolerance± mm | ±0.03 (Bambu Lab)[15] | Not documented |
| Printing Parameters | ||
| Nozzle temperature°C | 190–230 (Bambu Lab); 190–210 (Fiberlogy PLA Mineral)[2][1] | Not documented |
| Bed temperature°C | 35–45 (Bambu Lab); 60 (Fiberlogy)[2][1] | Not documented |
| Enclosure / chamber requirement1–5 | Open frame is fine[2][1] | Enclosure required (passive) — Polymaker states its Fiberon PPS-CF10 needs no heated chamber, unlike the unfilled sulfones and PAEKs[3] |
| Part cooling fan | Fan on; Fiberlogy specifies 75–100 %[2][1] | Not documented |
| Bed surface & adhesion aid | Cool plate, high-temperature plate or textured PEI with glue (Bambu Lab); smooth PEI, textured PEI or glass (Fiberlogy)[2][1] | Not documented |
| Warping tendency1–5 | None[2] | Not documented |
| Bed-adhesion difficulty1–5 | Sticks to anything[16] | Not documented |
| Overall printing difficulty1–5 | Beginner — prints on any machine out of the box[2][1] | Expert / industrial hardware only[3] |
| Hardware Wear & Reliability | ||
| Nozzle hardness required1–4 | Brass fine indefinitely[17][2][1] | Hardened steel required[3] |
| Abrasiveness1–5 | Slightly abrasive — mineral filler pushes density from 1.24 to 1.31–1.38[1][2][18] | Highly abrasive — standard CF composite[3] |
| Nozzle clog risk1–5 | Very low[17] | High — jams from moisture, heat creep or particles; Polymaker specifies hardened steel or ruby nozzles for carbon-filled PPS and Prusa lists composites as a higher clogging risk[19][20] |
| Heat-creep / jam sensitivity1–5 | Moderate — good heatbreak cooling needed; PLA softens below 60 °C[21] | Not documented |
| Hotend requirement | No special hot-end required[16] | Not documented |
| Moisture Behaviour | ||
| Moisture absorption (hygroscopicity)1–5 | Moderate — 0.40 % saturated at 25 °C / 55 % RH[2] | Low (0.1–0.3 %) — 0.225 % equilibrium for Fiberon PPS-CF10 and 0.11 % for PPS-GF20[3][4] |
| Equilibrium moisture content at ~50 % RH% | 0.40 saturated at 25 °C / 55 % RH (Bambu Lab)[2] | 0.225 equilibrium (Fiberon PPS-CF10); 0.11 (PPS-GF20)[3][4] |
| Drying temperature & time | 50 °C for 8 h in a forced-air dryer, or 60–70 °C for 12 h on an X1 heatbed; Fiberlogy specifies 50 °C for 6 h[2][1][22] | Not documented |
| Symptoms when wet | Bubbling and popping at the nozzle, stringing, rough surface and weak layers[23] | Not documented |
| Effect of moisture on strength | Polymaker rates PLA low-sensitivity — the loss shows as poor layer adhesion and brittle layers rather than a published strength figure[23] | No dry-versus-conditioned figures are published; equilibrium uptake is 0.225 % and Polymaker specifies a 100 °C, 10 h dry[3] |
| Storage requirement | Sealed with desiccant below 20 % RH; shelf life at ambient is long[18][16] | Not documented |
| Mechanical Properties | ||
| Tensile strength (XY)MPa | 30 (printed XY, ISO 527, Bambu Lab); 35.1 on My Tech Fun bars for PolyTerra PLA[2][24] | 59.4 ± 1.3 (PPS-CF10) and 64.1 ± 2.1 (PPS-GF20) printed XY, ISO 527[3][4] |
| Young's modulusMPa | 1960 (Bambu Lab, printed XY, ISO 527); Fiberlogy PLA Mineral quotes 3500 (ISO 527, specimen type not stated)[2][1] | 5446.7 ± 149.0 (PPS-CF10) and 4552.0 ± 54.6 (PPS-GF20) printed XY, ISO 527[3][4] |
| Elongation at break% | 14.8 (printed XY, ISO 527)[2] | 1.4 ± 0.1 (PPS-CF10) and 2.0 ± 0.2 (PPS-GF20) printed XY, ISO 527 — the lowest elongation in the dataset[3][4] |
| Flexural strengthMPa | 53 (printed XY, ISO 178) — 30 % below PLA Basic at 76[2][18] | Not documented |
| Flexural modulusMPa | 2360 (printed XY, ISO 178)[2] | Not documented |
| Charpy impact, notchedkJ/m² | 6.3 (printed XY, ISO 179, notched); unnotched 19.2[2] | 5.3 ± 0.2 printed XY for PPS-CF10 and 7.3 ± 0.2 for PPS-GF20, ISO 179 notched[3][4] |
| Other impact data | Izod 6.1 kJ/m² on My Tech Fun printed bars for PolyTerra PLA[24] | Not documented |
| Layer adhesion / Z tensileMPa | 22 (printed Z, ISO 527); flexural Z falls to 29 against 53 in XY; 12.9 on My Tech Fun layer-adhesion bars[2][24] | 32.0 ± 5.1 (PPS-CF10) and 22.9 ± 0.8 (PPS-GF20) printed Z, ISO 527[3][4] |
| Brittleness1–5 | Brittle — snaps with little warning[2] | Very brittle — cracks or shatters easily; elongation at break 1.4 %[3] |
| Hardness (scale-specific)Shore A / Shore D / Rockwell | Not documented | Rockwell 105 (and R124) on extruded unfilled PPS stock (ASTM D785); no figure is published for a fibre-filled PPS filament[25] |
| Creep resistance / sustained load1–5 | Poor — 12 mm bar sagged to 18.7 mm over 5 days at 1.25 kg[24] | Excellent — holds load for years. Ensinger lists high creep resistance for unfilled PPS stock and Spectrum states creep resistance is unchanged under continuous load at high temperature; the fibre raises heat deflection to 252 °C at 0.45 MPa[25][26][3] |
| Fatigue / repeated-flex resistance1–5 | Poor — no grade-specific S-N curve; plain printed PLA ran 38 000–49 000 cycles at 30 % of tensile strength (R = 0.2)[27][21] | Not documented |
| Elasticity / flexibility1–5 | Rigid[2] | Rigid[3] |
| Z strength as % of XY% | 73 by tensile, 55 by flexural (printed, Bambu Lab)[2] | 54 (PPS-CF10) and 36 (PPS-GF20), printed[3][4] |
| Thermal Properties | ||
| HDT at 0.45 MPa°C | 58 (Bambu Lab) and 48 (Fiberlogy PLA Mineral), ISO 75 at 0.45 MPa[2][1] | 252.5 (PPS-CF10) and 236.3 (PPS-GF20), printed, ISO 75 at 0.45 MPa[3][4] |
| HDT at 1.8 MPa°C | 52 (ISO 75, 1.8 MPa)[2] | 133 (PPS-CF10) and 125.8 (PPS-GF20), printed, ISO 75 at 1.8 MPa[3][4] |
| Glass transition (Tg)°C | 61 (DSC)[2] | 97.7 (PPS-CF10) and 95.0 (PPS-GF20), DSC[3][4] |
| Melting point / Vicat°C | 163 peak melt (DSC); Vicat 63 °C[2] | 279.7 (PPS-CF10) and 279.6 (PPS-GF20) melting, DSC; Vicat 267.5 and 272.5 (ISO 306)[3][4] |
| Continuous service temperature°C | 54 — loaded bars begin to move at this temperature[24] | 170 long-term service on extruded PPS stock, converted from 338 °F; no figure published for the carbon-filled grade[25] |
| Annealing response | 50–60 °C for 6–12 h; some prints deform or warp, and a forced-air oven is required[2] | Not documented |
| Flammability / UL 94 | Flammable; no UL 94 rating published by the major brands[18][28] | Not documented |
| Environment & Chemical | ||
| UV resistance1–5 | Degrades within weeks outdoors[21][29] | Not documented |
| Chemical resistance | Good against weak acids, oils and grease; poor against strong acids and alkalis; dissolved by chloroform, THF and hot benzene[28][21] | Outstanding — PPS resists essentially all solvents below 200 °C[19] |
| Water / humidity resistance in service1–5 | Good — insoluble in water[18] | Not documented |
| Food contact | Base resin is food-contact grade, but printed layer grooves harbour bacteria; Prusa advises against food use[21] | Not documented |
| Biodegradability / compostability | Industrially compostable only — needs sustained 55 °C; not home compostable[30][21] | Not documented |
| Recyclability | Mechanically recyclable; not accepted in household plastic collection[30] | Not documented |
| Electrical & ESD properties | Not documented | Surface resistivity above 10¹² ohm — insulating (ANSI/ESD S11.11)[3][4] |
| Health & Safety | ||
| Fume toxicity1–5 | Low hazard — minimal VOC and particle emission[31] | Moderate — measurable VOCs and UFPs, ventilation advised. None of these polymers was in the chamber study, and all are processed far above the temperatures it covered[31] |
| Ventilation / filtration requirement1–5 | None needed in a normal room[31] | Ventilated room or enclosure recommended[31] |
| Dust & fibre handling hazard | Not documented | Fibre is bound in the matrix; sanding dust should not be inhaled[3] |
| Post-Processing | ||
| Sanding & machining | Wet sanding — dry sanding heats the surface by friction and smears it[29][21] | Not documented |
| Gluing & solvent welding | Cyanoacrylate for most joints; some grades partially dissolve and bond with acetone[21][32] | Not documented |
| Vapour / chemical smoothing | No practical vapour smoothing — only chloroform, hot benzene or THF, which are laboratory-only[21] | Not documented |
| Support material pairing | Support for PLA (Bambu Lab)[2] | Not documented |
| Dimensional accuracy & detail | Matte surface hides layer lines; 55° overhangs and 30 mm bridges as for plain PLA[2] | Not documented |
| Solvents & Solubility | ||
| Soluble in | Chloroform: 10 % w/v in 2–4 h at 23 °C, every grade and morphology; THF and DMF only at 65 °C. Laboratory reagents.[33] | None — PPS does not dissolve in any known solvent below 200 °C.[34][35] |
| Softened or crazed by | Acetone, ethyl acetate and toluene plasticise it but dissolve <1 % even at 65 °C; submersion in acetone crazes and destroys parts.[33][36] | Nothing at 23 °C; Ensinger rates it only conditionally resistant to benzene, dichloromethane, toluene and pyridine.[35] |
| Solvent welding & smoothing agent | Chloroform vapour smooths and welds PLA at the cost of tensile strength; acetone does not smooth it at all.[37][36] | None — no solvent welds or smooths PPS.[34] |
Material entries describe families or representative grades, not an interchangeable specification for every spool. Test methods, orientations and conditions may differ. Unknown values are marked “Not documented”. Prices and source dates remain historical snapshots; check the linked guide for product details. Differences highlight text, not a universal winner.
Sources for this comparison
- PLA Mineral — product and technical data Fiberlogy · 2026-08 · tds
- Bambu Filament Technical Data Sheet V3.0 — PLA Matte Bambu Lab · 2026-08 · tds
- Fiberon PPS-CF10 Technical Data Sheet V1.1 Polymaker · 2025-07 · tds
- Fiberon PPS-GF20 Technical Data Sheet V1.1 Polymaker · 2025-07 · tds
- Polymaker Panchroma Matte PLA — product listing 3DJake International · 2026-08 · vendor
- Overture Matte PLA 1.75mm Overture3D · 2026-08 · vendor
- Matte PLA filament collection Anycubic Official Store · 2026-08 · vendor
- Polymaker product catalogue Polymaker · 2026-08 · vendor
- Bambu Lab PPS-CF Black, spool (750 g) 3DJAKE · 2026-08 · vendor
- 3D4Makers product catalogue 3D4Makers · 2026-08 · vendor
- IEMAI 3D CF-PPS 3D Printing Filament — store page IEMAI 3D · 2026-08 · vendor
- Matte PLA filament collection Sunlu Official Store · 2026-08 · vendor
- Fiberlogy PLA Mineral — product listing 3DJake International · 2026-08 · vendor
- Extrudr PLA NX2 Matt — product listing 3DJake International · 2026-08 · vendor
- PLA Basic — product page Bambu Lab US Store · 2026-08 · vendor
- PLA — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- Filament Material Guide Prusa Knowledge Base · 2026-08 · doc
- Bambu Filament Technical Data Sheet V3.0 — PLA Basic Bambu Lab · 2026-08 · tds
- PPS — material basics Polymaker Wiki · 2026-08 · doc
- Composite materials filled with carbon, kevlar or glass Prusa Knowledge Base · 2026-08 · doc
- PLA — material guide Prusa Knowledge Base · 2026-08 · doc
- Filament Drying Recommendations Bambu Lab Wiki · 2026-08 · doc
- Wet Filament — signs, causes and drying Polymaker Wiki · 2026-08 · doc
- PolyTerra PLA vs PLA+ — results spreadsheet My Tech Fun (Igor Gaspar) · 2026-08 · test
- TECATRON natural (PPS) — stock shape properties Ensinger · 2026-08 · tds
- Spectrum PPS AM230 Technical Data Sheet Spectrum Filaments · 2022-04 · tds
- Mechanical Properties of Additively Manufactured Polymeric Materials — PLA and PETG — For Biomechanical Applications Polymers 16(13):1868 · 2024-06 · paper
- PolyLite PLA Technical Data Sheet V5.4 Polymaker · 2024-11 · tds
- Prusament PLA Technical Data Sheet v1.0 Prusa Polymers · 2018-09 · tds
- Filamentive PLA (recycled) — product page Filamentive · 2026-08 · vendor
- Emissions of Ultrafine Particles and Volatile Organic Compounds from Commercially Available Desktop Three-Dimensional Printers with Multiple Filaments (Azimi et al.) Environmental Science & Technology 50(3) 1260-1268 · 2016-01 · paper
- Prusament rPLA Corn Pigment 1kg — product page Prusa Research · 2026-08 · vendor
- Solubility Study of Ingeo Biopolymer Grades in Common Organic Solvents (NWPD003) NatureWorks · 2019-10 · tds
- PPS (Polyphenylene sulfide) — Knowledge Base Prusa Research · 2026-08 · doc
- Chemical resistance — resistance of Ensinger plastics to chemicals (DIN 50 014, 23/50) Ensinger · 2026-08 · tds
- Improve your 3D prints with chemical smoothing Prusa Research · 2026-08 · doc
- Effect of vapour smoothing in trichloromethane on 3D printed PLA — surface, mechanical and chemical structure Pitale, Keche & Chopra, Engineering Research Express 6(4) 045579 · 2024-12 · paper