| Property | High-Speed PLAPLA | Stone-filled PLAPLA |
|---|---|---|
| Market snapshot | ||
| Listing priceUSD/kg; dated snapshots | $19.99/kg median; $11.49–$32.99/kg across 10 dated product listings | $22.99/kg median; $15.99–$49.16/kg across 6 dated product listings |
| Identity & Market | ||
| Base polymer / chemistry | PLA with rheology and crystallisation tuned for high volumetric flow; melt index 15.4 g/10 min vs 7–11 for standard PLA[1][2] | PLA filled with stone or mineral powder — Formfutura StoneFil declares 40–50 wt% stone powder[3][4] |
| Densityg/cm³ | 1.23 (ISO 1183, at 21.5 °C)[1] | 1.22 (Bambu Lab PLA Marble) and 1.50–1.70 (Formfutura StoneFil), ISO 1183[4][3] |
| Typical priceUSD/kg | Mainstream 1 kg spools cluster near 20[5][6][7] | 1 kg spools cluster near 21[8][9] |
| Price range across brandsUSD/kg | 11–33 across brands; budget house brands 11–18, Prusament 33[10][11][12] | 16–49 across brands; SUNLU 16, ELEGOO 19, Polymaker 21, Bambu Lab 25, Prusament 38, Filament PM MarbleJet 49 on 0.5 kg spools[13][9][8][14][15][16] |
| Market availability1–5 | Stocked by most mainstream brands[17][7][18] | Stocked by most mainstream brands[8][9][13] |
| Spool sizes & diameters | 1.75 mm; 1 kg spools[5][7] | 1.75 and 2.85 mm; 0.5 and 1 kg spools plus refills[9][3] |
| Typical applications | Large or repetitive prints on printers that can sustain high flow[19][17] | Architectural models, sculpture and props with a matte mineral surface[4] |
| Diameter tolerance± mm | ±0.03 (Bambu Lab PLA Basic, rated to 258 mm/s)[20] | Not documented |
| Printing Parameters | ||
| Nozzle temperature°C | 210–230 for high-speed work; 190–210 at classic speeds[1][17] | 190–230 (Bambu Lab)[4] |
| Bed temperature°C | 30–60 (Polymaker); 35–45 (Bambu Lab)[1][21] | 35–45 (Bambu Lab)[4] |
| Enclosure / chamber requirement1–5 | Open frame is fine[1] | Open frame is fine[4] |
| Part cooling fan | Fan on[1] | Fan on[4] |
| Maximum volumetric flow (mm³/s; see test conditions)mm³/s | ≈24 at 300 mm/s with a 0.4 mm nozzle and 0.2 mm layer; 30 % more flow than regular PLA at the same temperature[1][17][19][22] | Not documented |
| Warping tendency1–5 | None[1] | Not documented |
| Bed-adhesion difficulty1–5 | Sticks to anything[23] | Not documented |
| Overall printing difficulty1–5 | Easy — minor profile tuning; needs a printer that can actually reach the flow rate[17][1] | Easy — minor profile tuning; 0.2 mm nozzles are not usable[24] |
| Extruder requirement | Not documented | Nozzles below 0.4 mm are not compatible (Bambu Lab)[24] |
| Hardware Wear & Reliability | ||
| Nozzle hardness required1–4 | Brass fine indefinitely[25] | Brass acceptable; hardened steel for volume work — Bambu Lab's compatibility table says no hardened nozzle is needed while the note under the same table groups PLA Marble with particle-filled materials that should always use one[24] |
| Abrasiveness1–5 | Non-abrasive[26][25] | Moderately abrasive — stone fill[24][3] |
| Nozzle clog risk1–5 | Very low[25] | Moderate — needs dry filament and a clean nozzle[24] |
| Heat-creep / jam sensitivity1–5 | Moderate — good heatbreak cooling needed; PLA softens below 60 °C[27] | Not documented |
| Hotend requirement | No special hot-end required[23] | Not documented |
| Moisture Behaviour | ||
| Moisture absorption (hygroscopicity)1–5 | Moderate — 0.40 % equilibrium at 23 °C / 70 % RH[1] | Moderate — 0.44 % saturated at 25 °C / 55 % RH[4] |
| Equilibrium moisture content at ~50 % RH% | 0.40 equilibrium at 23 °C / 70 % RH (Polymaker PolySonic)[1] | 0.44 saturated at 25 °C / 55 % RH (Bambu Lab)[4] |
| Drying temperature & time | 55 °C for 6 h; 50 °C for 8 h (Bambu Lab)[1][21] | Not documented |
| Symptoms when wet | Bubbling and popping at the nozzle, stringing, rough surface and weak layers[28] | Not documented |
| Effect of moisture on strength | Polymaker rates PLA low-sensitivity — the loss shows as poor layer adhesion and brittle layers rather than a published strength figure[28] | Polymaker rates PLA low-sensitivity and publishes no dry-versus-conditioned figures for this grade; absorbed water flashes to steam and shows as bubbling and poor layer adhesion[28] |
| Storage requirement | Sealed with desiccant below 20 % RH; shelf life at ambient is long[21][23] | Not documented |
| Mechanical Properties | ||
| Tensile strength (XY)MPa | 43.9 at 300 mm/s and 46.0 at 46.7 mm/s (printed XY, ISO 527); 58.6 on My Tech Fun bars for Creality Hyper PLA[1][29] | 33 ± 4 printed XY, ISO 527 (Bambu Lab)[4] |
| Young's modulusMPa | 2650 at 300 mm/s, 2878 at classic speed (printed XY, ISO 527)[1] | 2330 ± 240 printed XY, ISO 527 (Bambu Lab)[4] |
| Elongation at break% | 15.1 at 300 mm/s, 21.5 at classic speed (printed XY, ISO 527)[1] | 6.7 ± 0.5 printed XY, ISO 527 (Bambu Lab)[4] |
| Flexural strengthMPa | 71.4 at 300 mm/s, 76.5 at classic speed (printed XY, ISO 178)[1] | 75 ± 5 printed XY, ISO 178 (Bambu Lab)[4] |
| Flexural modulusMPa | 2798 at 300 mm/s, 2868 at classic speed (printed XY, ISO 178)[1] | 2920 ± 180 printed XY, ISO 178 (Bambu Lab)[4] |
| Charpy impact, notchedkJ/m² | 5.0 at 300 mm/s, 6.1 at classic speed (printed XY, ISO 179, notched)[1] | 9.5 ± 2.6 printed XY, ISO 179, notched (Bambu Lab)[4] |
| Other impact data | Printing at 300 mm/s instead of 46.7 mm/s costs 4.6 % tensile strength and 18 % notched Charpy[1] | Charpy unnotched 24.0 printed XY (Bambu Lab, ISO 179)[4] |
| Layer adhesion / Z tensileMPa | 32.4 at 300 mm/s, 37.3 at classic speed (printed Z, ISO 527); 35.3 for Creality Hyper PLA vs 23.0 for average PLA on identical bars[1][29] | 30 ± 4 printed Z, ISO 527 (Bambu Lab)[4] |
| Brittleness1–5 | Moderate[1] | Brittle — snaps with little warning[4] |
| Hardness (scale-specific)Shore A / Shore D / Rockwell | 78.7 Shore D measured on printed bars for Sunlu PLA Meta (My Tech Fun), against 75.3 for the same maker's plain PLA[30] | Not documented |
| Creep resistance / sustained load1–5 | Poor — 12 mm bar sagged to 17.7 mm over 6 days at 1.25 kg[29] | Poor — no stone-filled creep test; plain printed PLA sagged from 12 to 16.2–21.8 mm over 5 days at 1.25 kg[31][32][30] |
| Fatigue / repeated-flex resistance1–5 | Poor — no grade-specific S-N curve; plain printed PLA ran 38 000–49 000 cycles at 30 % of tensile strength (R = 0.2)[33][27] | Poor — no grade-specific S-N curve; plain printed PLA ran 38 000–49 000 cycles at 30 % of tensile strength and the mineral filler leaves a brittle compound[33][4] |
| Elasticity / flexibility1–5 | Rigid[1] | Rigid[4] |
| Z strength as % of XY% | 74 at 300 mm/s, 81 at classic speed (printed)[1] | 91 by tensile, 73 by flexural (printed, Bambu Lab)[4] |
| Thermal Properties | ||
| HDT at 0.45 MPa°C | 53 (ISO 75, 0.45 MPa)[1] | 56 (ISO 75, 0.45 MPa)[4] |
| HDT at 1.8 MPa°C | 52 (ISO 75, 1.8 MPa)[1] | 53 (ISO 75, 1.8 MPa)[4] |
| Glass transition (Tg)°C | 59 (DSC)[1] | 56 (DSC)[4] |
| Melting point / Vicat°C | 164 peak melt (DSC); crystallisation 96 °C, Vicat 61 °C[1] | 156 peak melt (DSC); Formfutura gives a 120–170 melting range for StoneFil[4][3] |
| Continuous service temperature°C | 53 — loaded bars begin to move at this temperature[29] | Not documented |
| Thermal expansion (CTE)µm/m·K | 96–99 for plain printed PLA (fibre Bragg grating, 25–50 °C); no grade-specific measurement published[34] | Not documented |
| Flammability / UL 94 | Flammable; no UL 94 rating published by the major brands[21][2] | Not documented |
| Environment & Chemical | ||
| UV resistance1–5 | Degrades within weeks outdoors[27][35] | Degrades within weeks outdoors[27] |
| Chemical resistance | Good against weak acids, oils and grease; poor against strong acids and alkalis[1] | Not documented |
| Water / humidity resistance in service1–5 | Good — insoluble in water[21] | Not documented |
| Food contact | Base resin is food-contact grade, but printed layer grooves harbour bacteria; Prusa advises against food use[27] | Not documented |
| Biodegradability / compostability | Industrially compostable only — needs sustained 55 °C; not home compostable[36][27] | Not documented |
| Recyclability | Mechanically recyclable; not accepted in household plastic collection[36] | Not documented |
| Health & Safety | ||
| Fume toxicity1–5 | Low hazard — minimal VOC and particle emission[37] | Low hazard — minimal VOC and particle emission[37] |
| Ventilation / filtration requirement1–5 | None needed in a normal room[37] | None needed in a normal room[37] |
| Dust & fibre handling hazard | Not documented | Formfutura's SDS sets an occupational limit of 1 mg/m³ for the stone powder and lists it as both a fibre and a particulate — do not dry-sand without extraction[3] |
| Post-Processing | ||
| Sanding & machining | Wet sanding — dry sanding heats the surface by friction and smears it[35][27] | Sands to a stone-like matte surface[3] |
| Gluing & solvent welding | Cyanoacrylate for most joints; some grades partially dissolve and bond with acetone[27][38] | Not documented |
| Vapour / chemical smoothing | No practical vapour smoothing — only chloroform, hot benzene or THF, which are laboratory-only[27] | Not documented |
| Support material pairing | PolySupport and PolyDissolve S1 (Polymaker)[1] | Support for PLA (Bambu Lab)[4] |
| Dimensional accuracy & detail | Not documented | Matte mineral surface hides layer lines; 55° overhangs and 30 mm bridges as for plain PLA[4] |
| Solvents & Solubility | ||
| Soluble in | Chloroform: 10 % w/v in 2–4 h at 23 °C, every grade and morphology; THF and DMF only at 65 °C. Laboratory reagents.[39] | Chloroform dissolves the PLA matrix (10 % w/v, 2–4 h at 23 °C) and leaves the filler as loose sludge; laboratory reagent.[39] |
| Softened or crazed by | Acetone, ethyl acetate and toluene plasticise it but dissolve <1 % even at 65 °C; submersion in acetone crazes and destroys parts.[39][40] | Acetone, ethyl acetate and toluene plasticise the matrix but dissolve <1 % even at 65 °C; acetone submersion crazes parts.[39][40] |
| Solvent welding & smoothing agent | Chloroform vapour smooths and welds PLA at the cost of tensile strength; acetone does not smooth it at all.[41][40] | Chloroform vapour attacks only the resin fraction, so the filler is left standing proud; no workshop-safe agent exists.[41][40] |
Material entries describe families or representative grades, not an interchangeable specification for every spool. Test methods, orientations and conditions may differ. Unknown values are marked “Not documented”. Prices and source dates remain historical snapshots; check the linked guide for product details. Differences highlight text, not a universal winner.
Sources for this comparison
- PolySonic PLA Technical Data Sheet V5.4 Polymaker · 2024-11 · tds
- PolyLite PLA Technical Data Sheet V5.4 Polymaker · 2024-11 · tds
- StoneFil safety data sheet Formfutura · 2026-08 · msds
- Bambu Filament Technical Data Sheet — PLA Marble Bambu Lab · 2026-08 · tds
- PolySonic PLA 1.75mm/1kg — product page Polymaker Shop · 2026-08 · vendor
- Overture High Speed PLA 1.75mm Overture3D · 2026-08 · vendor
- High Speed PLA filament collection Anycubic Official Store · 2026-08 · vendor
- PLA Marble — product page Bambu Lab US Store · 2026-08 · vendor
- Polymaker product catalogue Polymaker · 2026-08 · vendor
- PLA Meta filament collection Sunlu Official Store · 2026-08 · vendor
- QIDI PLA Rapido 1.75mm 1kg 3D Printers Depot · 2026-08 · vendor
- Prusament PLA Prusa Pro Green 1kg (NFC) Prusa Research · 2026-08 · vendor
- ELEGOO product catalogue ELEGOO · 2026-08 · vendor
- Printed Solid product catalogue Printed Solid · 2026-08 · vendor
- SUNLU High Speed PLA Marble 3D Printer Filament 1 kg SUNLU · 2026-08 · vendor
- Filament PM PLA MarbleJet technical data sheet Filament PM (Plasty Mladec) · 2026-08 · tds
- PolySonic PLA — product page Polymaker · 2026-08 · vendor
- Creality PLA filament collection Creality Official Store · 2026-08 · vendor
- Polymaker Launches New High-Speed 3D Printing Filament — PolySonic PLA & PLA Pro Polymaker · 2023-11 · doc
- PLA Basic — product page Bambu Lab US Store · 2026-08 · vendor
- Bambu Filament Technical Data Sheet V3.0 — PLA Basic Bambu Lab · 2026-08 · tds
- Max volumetric speed Prusa Knowledge Base · 2026-08 · doc
- PLA — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- PLA Usage Guide Bambu Lab Wiki · 2026-08 · doc
- Filament Material Guide Prusa Knowledge Base · 2026-08 · doc
- Prusament PLA — material page Prusa Polymers · 2026-08 · doc
- PLA — material guide Prusa Knowledge Base · 2026-08 · doc
- Wet Filament — signs, causes and drying Polymaker Wiki · 2026-08 · doc
- Creality Hyper PLA filament review — results spreadsheet My Tech Fun (Igor Gaspar) · 2026-08 · test
- Carbon Fiber PLA vs META-PLA vs PLA+ vs PLA by Sunlu — results spreadsheet My Tech Fun (Igor Gaspar) · 2026-08 · test
- BambuLab PLA Basic vs PLA Tough vs PLA-CF — results spreadsheet My Tech Fun (Igor Gaspar) · 2026-08 · test
- Polymaker PLA Pro vs PLA-CF — results spreadsheet My Tech Fun (Igor Gaspar) · 2026-08 · test
- Mechanical Properties of Additively Manufactured Polymeric Materials — PLA and PETG — For Biomechanical Applications Polymers 16(13):1868 · 2024-06 · paper
- Characterization of Thermal Expansion Coefficient of 3D Printing Polymeric Materials Using Fiber Bragg Grating Sensors Materials 17(18):4668 · 2024-09 · paper
- Prusament PLA Technical Data Sheet v1.0 Prusa Polymers · 2018-09 · tds
- Filamentive PLA (recycled) — product page Filamentive · 2026-08 · vendor
- Emissions of Ultrafine Particles and Volatile Organic Compounds from Commercially Available Desktop Three-Dimensional Printers with Multiple Filaments (Azimi et al.) Environmental Science & Technology 50(3) 1260-1268 · 2016-01 · paper
- Prusament rPLA Corn Pigment 1kg — product page Prusa Research · 2026-08 · vendor
- Solubility Study of Ingeo Biopolymer Grades in Common Organic Solvents (NWPD003) NatureWorks · 2019-10 · tds
- Improve your 3D prints with chemical smoothing Prusa Research · 2026-08 · doc
- Effect of vapour smoothing in trichloromethane on 3D printed PLA — surface, mechanical and chemical structure Pitale, Keche & Chopra, Engineering Research Express 6(4) 045579 · 2024-12 · paper