Filament comparison
PEKK vs PLA Silk
Compare printing settings, strength, heat resistance, dated prices and sources.
2 selected · all documented properties
| Property | PEKKHIGHTEMP | Silk PLAPLA |
|---|---|---|
| Market snapshot | ||
| Listing priceUSD/kg; dated snapshots | $525.00/kg median; $332.50–$771.12/kg across 6 dated product listings | $19.49/kg median; $9.75–$24.99/kg across 15 dated product listings |
| Identity & Market | ||
| Base polymer / chemistry | Polyether ketone ketone, amorphous grade — a polyaryletherketone that stays amorphous, so it does not need PEEK's crystallisation control. Stratasys sells it as Antero 800NA and Antero 840CN03; category numbers below are unfilled unless a carbon grade is named[1][2] | PLA with a gloss-forming additive package; suppliers publish the composition as polylactic acid only[3] |
| Densityg/cm³ | 1.28 unfilled (ASTM D792, Antero 800NA; 1.31 annealed) and 1.33 for CarbonX PEKK-A CF15 (ISO 1183)[2][1] | 1.27 (ISO 1183)[3] |
| Typical priceUSD/kg | 1 kg-equivalent spools cluster near 550[4][5][6] | Mainstream 1 kg spools cluster near 20[7][8][9] |
| Price range across brandsUSD/kg | 333-771 across grades and formats; 3DXTech CarbonX PEKK-A+CF15 333 at 2 kg, 3D4Makers unfilled PEKK-A 485 at 2 kg, IEMAI 3D 500 at 1 kg, Kimya PEKK Carbon 771 at 500 g[4][5][6][10][11] | 10–25 across brands; CHCKX 10 in a 16-roll bundle, SUNLU 13, LANDU 18, YXPOLYER 20, Polymaker 22, Devil Design 25[12][13][14][15][16] |
| Market availability1–5 | Niche, a handful of specialist brands[4][5][6] | Stocked by most mainstream brands[7][12][17] |
| Spool sizes & diameters | 1.75 and 2.85 mm; 200 g to 2 kg spools, plus Stratasys canisters[4][5][2] | 1.75 mm; 1 and 1.1 kg spools; dual- and tri-colour coextruded variants[18][19] |
| Typical applications | Aerospace interior and structural parts; 3DXTech labels its carbon-filled PEKK-A grade AERO and Stratasys certifies Antero 800NA for outgassing and FST[1][2] | Decorative prints where surface gloss matters more than strength[3] |
| Diameter tolerance± mm | Not documented | ±0.03 (Bambu Lab)[20] |
| Printing Parameters | ||
| Nozzle temperature°C | Not documented | 210–240 — 20 °C above the plain PLA window[3] |
| Bed temperature°C | 140 (3DXTech CarbonX PEKK-A CF15)[1] | 35–45[3] |
| Enclosure / chamber requirement1–5 | Actively heated chamber required[21][22] | Open frame is fine[3][23] |
| Part cooling fan | Not documented | Fan on[3] |
| Bed surface & adhesion aid | Not documented | Cool Plate SuperTack, smooth PEI or textured PEI[3] |
| Warping tendency1–5 | Not documented | None[3] |
| Bed-adhesion difficulty1–5 | Not documented | Sticks to anything[24] |
| Overall printing difficulty1–5 | Expert / industrial hardware only[21][22] | Easy — minor profile tuning; hotter nozzle and slower cap of 250 mm/s[3] |
| Hardware Wear & Reliability | ||
| Nozzle hardness required1–4 | Hardened steel required — the category spans unfilled PEKK, where brass is acceptable, and the carbon-filled aerospace grades that make up most of the market[1][2] | Brass fine indefinitely[23] |
| Abrasiveness1–5 | Highly abrasive — most PEKK filament sold is carbon-filled; unfilled Antero 800NA and ThermaX PEKK-A are non-abrasive[1][2] | Non-abrasive[25][23] |
| Nozzle clog risk1–5 | Moderate — needs dry filament and a clean nozzle; 3DXTech lists no special nozzle concerns but a mandatory 120 °C pre-dry before every print[26] | Very low[23] |
| Heat-creep / jam sensitivity1–5 | Not documented | Moderate — good heatbreak cooling needed; PLA softens below 60 °C[27] |
| Hotend requirement | Not documented | No special hot-end required[24] |
| Moisture Behaviour | ||
| Moisture absorption (hygroscopicity)1–5 | Not documented | Moderate — 0.40 % saturated at 25 °C / 55 % RH[3] |
| Equilibrium moisture content at ~50 % RH% | Not documented | 0.40 saturated at 25 °C / 55 % RH (Bambu Lab)[3] |
| Drying temperature & time | Not documented | 55 °C for 8 h in a forced-air dryer, or 65–75 °C for 12 h on an X1 heatbed[3][28] |
| Symptoms when wet | Not documented | Bubbling and popping at the nozzle, stringing, rough surface and weak layers[29] |
| Effect of moisture on strength | No dry-versus-conditioned figures are published; 3DXTech mandates a 120 °C, 4 h pre-dry before every print because trapped water flashes to steam at these nozzle temperatures[26] | Polymaker rates PLA low-sensitivity — the loss shows as poor layer adhesion and brittle layers rather than a published strength figure[29] |
| Storage requirement | Not documented | Sealed with desiccant below 20 % RH; shelf life at ambient is long[30][24] |
| Mechanical Properties | ||
| Tensile strength (XY)MPa | 86.7-90.0 at yield and 73.0 at break (printed XZ, ASTM D638, Antero 800NA on the F900 and Fortus 450mc); 88.8 at break annealed; 126 at break for CarbonX PEKK-A CF15 (printed XY, ISO 527)[2][1] | 33 (printed XY, ISO 527); eSun Silk broke 22 % below the 16-brand PLA mean on identical 4×4 mm bars[3][31] |
| Young's modulusMPa | 2640-3870 (printed XZ, ASTM D638, Antero 800NA; upper figure annealed); 9125 for CarbonX PEKK-A CF15 (printed XY, ISO 527)[2][1] | 2130 (printed XY, ISO 527)[3] |
| Elongation at break% | 6.1 at break (printed XZ, ASTM D638, Antero 800NA); 2.3 in ZX; 3.15 for CarbonX PEKK-A CF15 (ISO 527)[2][1] | 2.8 (printed XY, ISO 527) — a quarter of PLA Basic at 12.2[3][30] |
| Flexural strengthMPa | 136 at 5 % strain (printed XZ, ASTM D790, Antero 800NA); 178 for CarbonX PEKK-A CF15 (printed XY, ISO 178)[2][1] | 75 (printed XY, ISO 178)[3] |
| Flexural modulusMPa | 3200 (printed XZ, ASTM D790, Antero 800NA); 8817 for CarbonX PEKK-A CF15 (printed XY, ISO 178)[2][1] | 2460 (printed XY, ISO 178)[3] |
| Charpy impact, notchedkJ/m² | Not documented | 10.3 (printed XY, ISO 179, notched); unnotched 18.5[3] |
| Other impact data | Izod notched 41.1 J/m XZ and 33.3 J/m ZX; unnotched 1730 J/m XZ against 203 J/m ZX (printed, ASTM D256/D4812, Antero 800NA)[2] | Not documented |
| Layer adhesion / Z tensileMPa | 50.1-59.4 at yield (printed ZX, ASTM D638, Antero 800NA); 56.0 for the ESD grade Antero 840CN03[2][32] | 25 (printed Z, ISO 527), and flexural Z collapses to 30 against 75 in XY; eSun Silk broke at 12.3 kg where twelve of the 16 plain PLAs managed 44.6–61.5 kg[3][31][33] |
| Brittleness1–5 | Moderate unfilled — 6.1 % elongation at break in plane; brittle in the carbon-filled grades at 3.15 %[2][1] | Brittle — snaps with little warning[3] |
| Creep resistance / sustained load1–5 | Excellent — holds load for years. Antero 800NA still holds 82 % of its room-temperature ZX tensile strength at 104 °C and 63 % at 132 °C (printed, ASTM D638)[2] | Poor — no silk-specific creep data published; plain PLA sagged from 12 to 18.7–20.3 mm over 5 days at 1.25 kg[34][35] |
| Fatigue / repeated-flex resistance1–5 | Not documented | Poor — no grade-specific S-N curve; plain printed PLA ran 38 000–49 000 cycles at 30 % of tensile strength (R = 0.2)[36][27] |
| Elasticity / flexibility1–5 | Rigid[1] | Rigid[3] |
| Z strength as % of XY% | 56-82 (Antero 800NA and 840CN03 printed on the F900 and Fortus 450mc, ZX against XZ tensile yield and break, ASTM D638)[2][32] | 76 by tensile, 40 by flexural (printed, Bambu Lab)[3] |
| Thermal Properties | ||
| HDT at 0.45 MPa°C | 158 (printed XY and ZX, ASTM D648 Method B at 66 psi, Antero 800NA); 285 for CarbonX PEKK-A CF15 (ISO 75 at 0.45 MPa)[2][1] | 60 (ISO 75, 0.45 MPa)[3] |
| HDT at 1.8 MPa°C | 156-157 (printed, ASTM D648 Method B at 264 psi, Antero 800NA); moulded 147[2] | 56 (ISO 75, 1.8 MPa)[3] |
| Glass transition (Tg)°C | 156 (ASTM D7426, Antero 800NA); 165 for CarbonX PEKK-A CF15 (DSC)[2][1] | 57 (DSC)[3] |
| Melting point / Vicat°C | 300 melt point (ASTM D7426 peak heat, Antero 800NA); 305 for CarbonX PEKK-A CF15 (DSC)[2][1] | 158 peak melt (DSC); Vicat 66 °C[3] |
| Continuous service temperature°C | Not documented | 50 — a loaded bar begins to move at this temperature (My Tech Fun, eSun eSilk PLA)[33] |
| Annealing response | Not documented | 50–55 °C for 6–12 h[3] |
| Thermal expansion (CTE)µm/m·K | 36.1 in XY and 50.2 in ZX (printed, 40-140 °C, ASTM E831, Antero 800NA); 47.4 and 51.2 for the ESD grade Antero 840CN03[2][32] | Not documented |
| Flammability / UL 94 | Not documented | Flammable; no UL 94 rating published by the major brands[30][37] |
| Environment & Chemical | ||
| UV resistance1–5 | Good — years with some colour shift. 1000 h of QUV cycling to ASTM G154 left Antero 800NA's yield strength unchanged at 57 MPa and raised stress at break 3.6 %[2] | Degrades within weeks outdoors[27][38] |
| Chemical resistance | Not documented | Good against weak acids, oils and grease; poor against strong acids and alkalis; dissolved by chloroform, THF and hot benzene[37][27] |
| Water / humidity resistance in service1–5 | Not documented | Good — insoluble in water[30] |
| Food contact | Not documented | Base resin is food-contact grade, but printed layer grooves harbour bacteria; Prusa advises against food use[27] |
| Biodegradability / compostability | Not documented | Industrially compostable only — needs sustained 55 °C; not home compostable[39][27] |
| Recyclability | Not documented | Mechanically recyclable; not accepted in household plastic collection[39] |
| Electrical & ESD properties | Unfilled PEKK is an insulator at above 1.4e14 ohm-cm (ASTM D257); CarbonX PEKK-A CF15 sits above 10^7 ohm/sq, and the Antero 840CN03 ESD grade is specified at 10^4-10^9 ohm-cm[2][1][32] | Not documented |
| Health & Safety | ||
| Fume toxicity1–5 | Moderate — measurable VOCs and UFPs, ventilation advised. None of these polymers was in the chamber study, and all are processed far above the temperatures it covered[40] | Low hazard — minimal VOC and particle emission[40] |
| Ventilation / filtration requirement1–5 | Ventilated room or enclosure recommended[40] | None needed in a normal room[40] |
| Dust & fibre handling hazard | Carbon fibre is bound in the matrix; sanding dust should not be inhaled[1] | Not documented |
| Post-Processing | ||
| Sanding & machining | Not documented | Wet sanding — dry sanding heats the surface by friction and smears it[38][27] |
| Gluing & solvent welding | Not documented | Cyanoacrylate for most joints; some grades partially dissolve and bond with acetone[27][41] |
| Vapour / chemical smoothing | Not documented | No practical vapour smoothing — only chloroform, hot benzene or THF, which are laboratory-only[27] |
| Support material pairing | Not documented | Support for PLA (Bambu Lab)[3] |
| Dimensional accuracy & detail | Not documented | 55° overhangs and 30 mm bridges; gloss hides fine detail and is destroyed by sanding[3] |
| Solvents & Solubility | ||
| Soluble in | Concentrated sulphuric acid, as for PEEK; no common organic solvent touches a polyaryletherketone.[42][43] | Chloroform: 10 % w/v in 2–4 h at 23 °C, every grade and morphology; THF and DMF only at 65 °C. Laboratory reagents.[44] |
| Softened or crazed by | Concentrated sulphuric acid and liquid Freon are the entries Ensinger marks not resistant; acetone, MEK and toluene do nothing.[42] | Acetone, ethyl acetate and toluene plasticise it but dissolve <1 % even at 65 °C; submersion in acetone crazes and destroys parts.[44][45] |
| Solvent welding & smoothing agent | None — no solvent softens a polyaryletherketone.[42] | Chloroform vapour smooths and welds PLA at the cost of tensile strength; acetone does not smooth it at all.[46][45] |
Material entries describe families or representative grades, not an interchangeable specification for every spool. Test methods, orientations and conditions may differ. Unknown values are marked “Not documented”. Prices and source dates remain historical snapshots; check the linked guide for product details. Differences highlight text, not a universal winner.
Sources for this comparison
- CarbonX Carbon Fiber PEKK-A CF15 Technical Data Sheet v1 3DXTech · 2026-08 · tds
- Antero 800NA — FDM Material Data Sheet (PEKK-based) Stratasys · 2025-08 · tds
- Bambu Filament Technical Data Sheet V1.0 — PLA Silk+ Bambu Lab · 2026-08 · tds
- 3DXTech product catalogue 3DXTech · 2026-08 · vendor
- 3D4Makers product catalogue 3D4Makers · 2026-08 · vendor
- Kimya PEKK-A Natural 1.75 mm 500 g igo3d · 2026-08 · vendor
- Panchroma Silk PLA collection Polymaker Shop · 2026-08 · vendor
- Spectrum PLA Silk — product listing 3DJake International · 2026-08 · vendor
- 3DJake ecoPLA Silk Black 1.75mm 1000g 3DJake International · 2026-08 · vendor
- Kimya PEKK Carbon Grey 1.75 mm 500 g igo3d · 2026-08 · vendor
- IEMAI 3D PEKK 3D Printing Filament — store page IEMAI 3D · 2026-08 · vendor
- Sunlu Silk PLA+ 1.75mm 1kg Sunlu Official Store · 2026-08 · vendor
- Bambu Lab PLA Silk 1.75mm 1kg 3D Universe · 2026-08 · vendor
- CHCKX 16 Pack Silk Dual Color PLA Filament Bundle CHCKX (Amazon US) · 2026-08 · vendor
- YXPOLYER Silk PLA Black&Gold product page YXPOLYER · 2026-08 · vendor
- LANDU Silk Tri-Color PLA Filament 1.75 mm 1 kg LANDU (Amazon US) · 2026-08 · vendor
- Overture Silk PLA 1.75mm Overture3D · 2026-08 · vendor
- eSUN PLA-Silk Magic 1.75mm eSUN Official Store · 2026-08 · vendor
- JAYO Silk PLA+ 1.75mm 1.1kg JAYO Official Store · 2026-08 · vendor
- PLA Basic — product page Bambu Lab US Store · 2026-08 · vendor
- Prusament PEI 1010 Technical Datasheet v1.0 Prusa Polymers · 2024-09 · tds
- Prusament PEI 1010 — material page Prusa Polymers · 2026-08 · doc
- Filament Material Guide Prusa Knowledge Base · 2026-08 · doc
- PLA — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- Prusament PLA — material page Prusa Polymers · 2026-08 · doc
- THERMAX PEKK-A — product page (print recommendations) 3DXTech · 2026-08 · doc
- PLA — material guide Prusa Knowledge Base · 2026-08 · doc
- Filament Drying Recommendations Bambu Lab Wiki · 2026-08 · doc
- Wet Filament — signs, causes and drying Polymaker Wiki · 2026-08 · doc
- Bambu Filament Technical Data Sheet V3.0 — PLA Basic Bambu Lab · 2026-08 · tds
- 16 PLA brand comparison test — results spreadsheet My Tech Fun (Igor Gaspar) · 2022-10 · test
- Antero 840CN03 — FDM Material Data Sheet (PEKK, ESD) Stratasys · 2024-08 · tds
- Testing eSun PLA filaments: PLA-ST vs PLA+ vs Silk PLA My Tech Fun (Igor Gaspar) · 2026-08 · test
- BambuLab PLA Basic vs PLA Tough vs PLA-CF — results spreadsheet My Tech Fun (Igor Gaspar) · 2026-08 · test
- PolyTerra PLA vs PLA+ — results spreadsheet My Tech Fun (Igor Gaspar) · 2026-08 · test
- Mechanical Properties of Additively Manufactured Polymeric Materials — PLA and PETG — For Biomechanical Applications Polymers 16(13):1868 · 2024-06 · paper
- PolyLite PLA Technical Data Sheet V5.4 Polymaker · 2024-11 · tds
- Prusament PLA Technical Data Sheet v1.0 Prusa Polymers · 2018-09 · tds
- Filamentive PLA (recycled) — product page Filamentive · 2026-08 · vendor
- Emissions of Ultrafine Particles and Volatile Organic Compounds from Commercially Available Desktop Three-Dimensional Printers with Multiple Filaments (Azimi et al.) Environmental Science & Technology 50(3) 1260-1268 · 2016-01 · paper
- Prusament rPLA Corn Pigment 1kg — product page Prusa Research · 2026-08 · vendor
- Chemical resistance — resistance of Ensinger plastics to chemicals (DIN 50 014, 23/50) Ensinger · 2026-08 · tds
- The Effects of Sulfonated Poly(ether ether ketone) Ion Exchange Preparation Conditions on Membrane Properties Yee, Zhang & Ladewig, Membranes 3(3) 182–195 · 2013-07 · paper
- Solubility Study of Ingeo Biopolymer Grades in Common Organic Solvents (NWPD003) NatureWorks · 2019-10 · tds
- Improve your 3D prints with chemical smoothing Prusa Research · 2026-08 · doc
- Effect of vapour smoothing in trichloromethane on 3D printed PLA — surface, mechanical and chemical structure Pitale, Keche & Chopra, Engineering Research Express 6(4) 045579 · 2024-12 · paper