| Property | PEBA (polyether block amide)FLEX | PETGPETG |
|---|---|---|
| Market snapshot | ||
| Listing priceUSD/kg; dated snapshots | $60.99/kg median; $60.99–$60.99/kg across 1 dated product listings | $19.99/kg median; $8.99–$69.99/kg across 21 dated product listings |
| Identity & Market | ||
| Base polymer / chemistry | Polyether block amide: rigid polyamide and flexible polyether blocks.[1] | Polyethylene terephthalate glycol copolymer — PET with a glycol comonomer that suppresses crystallisation[2][3] |
| Densityg/cm³ | 1.01 g/cm³ (GB/T 1033; eSUN manufacturer data)[1] | 1.24–1.30 (ISO 1183)[2][3][4][5] |
| Typical priceUSD/kg | Not documented | 1 kg spools cluster near 20[6][7][8] |
| Price range across brandsUSD/kg | Not documented | 12–70 across brands; IEMAI 12, ELEGOO 14, CHCKX 14, Bambu Lab 18–20, Hatchbox 26, Prusament 38, Prusament PETG V0 70[6][7][9][8][10][11] |
| Market availability1–5 | Not documented | Ubiquitous, every brand and retailer[6][7][12][8] |
| Spool sizes & diameters | 1.75 mm diameter, 1 kg spool.[13] | 1.75 and 2.85 mm; 0.75, 0.8 and 1 kg spools plus spool-less refills[7][8] |
| Typical applications | Manufacturer applications include footwear, sports equipment and cushioning.[1] | Functional parts, enclosures and outdoor fittings that need more toughness and heat tolerance than PLA[2][3] |
| Diameter tolerance± mm | Not documented | ±0.02 (Prusament)[2] |
| Printing Parameters | ||
| Nozzle temperature°C | 230–260 °C; 240 °C recommended.[1] | 230–260 across brands; Prusament 250 ± 10, Polymaker 240–260[2][3][5] |
| Bed temperature°C | 60–90 °C[1] | 60–90; Prusament 80 ± 10, Polymaker 60–70[2][5] |
| Enclosure / chamber requirement1–5 | Not documented | Open frame is fine[5] |
| Part cooling fan | 10–50% fan recommended; mechanical-test specimens used 50–100%.[1] | Around 50 %; Polymaker specifies 20–60 %, less than PLA to protect layer bonding[2][5] |
| Bed surface & adhesion aid | PEI build plate[1] | Textured PEI, satin or powder-coated sheets. On smooth PEI a glue stick is used as a release agent, not an adhesive — PETG bonds to bare PEI hard enough to tear the sheet[2][5] |
| Maximum volumetric flow (mm³/s; see test conditions)mm³/s | 9 mm³/s maximum in eSUN spiral-vase test; mechanical specimens used 2 mm³/s. Linear recommendation 25–110 mm/s is a separate quantity.[1] | 8–15 (PrusaSlicer guidance); My Tech Fun ran Bambu Lab PETG Basic at 13 mm³/s[14][15] |
| Warping tendency1–5 | Not documented | Slight — corner lift on large flat parts[2][5] |
| Bed-adhesion difficulty1–5 | Not documented | Needs the right surface or a thin adhesive — the problem is releasing the part, not sticking it[2] |
| Stringing / oozing tendency1–5 | Not documented | Moderate — retraction tuning needed[2][5] |
| Overall printing difficulty1–5 | Not documented | Easy — minor profile tuning[5] |
| Hardware Wear & Reliability | ||
| Nozzle hardness required1–4 | Not documented | Brass fine indefinitely[14] |
| Abrasiveness1–5 | Not documented | Non-abrasive[5] |
| Nozzle clog risk1–5 | Not documented | Low — no special hot-end required and clogging is not among the listed drawbacks; Prusa lists no drybox and no hardened nozzle[16][17] |
| Heat-creep / jam sensitivity1–5 | Not documented | Slightly sensitive[16] |
| Hotend requirement | Not documented | No special hot-end required[16] |
| Moisture Behaviour | ||
| Moisture absorption (hygroscopicity)1–5 | Not documented | Moderate (0.3–0.8 %) — Bambu Lab reports 0.40 % saturated at 25 °C / 55 % RH; Prusa measures only 0.07 % in 24 h and 0.10 % in 7 days at the drier 22 % RH[2][18] |
| Equilibrium moisture content at ~50 % RH% | Not documented | 0.10 after 7 days at 24 °C / 22 % RH (Prusa Polymers); 0.40 saturated at 25 °C / 55 % RH (Bambu Lab)[2][18] |
| Drying temperature & time | 70–75 °C for 6–8 h; re-dry after receiving or extended exposure.[1] | 60–65 °C for 6–8 h[5][18] |
| Symptoms when wet | Not documented | Bubbling and popping at the nozzle, stringing and a rough surface[2] |
| Effect of moisture on strength | Not documented | Polymaker groups PETG with nylon, PVA and TPU as highly hygroscopic and shows a before-and-after-drying comparison; the loss appears as poor layer adhesion and weak, brittle layers rather than a published dry-versus-conditioned figure[19] |
| Storage requirement | Not documented | Sealed with desiccant; Polymaker groups PETG with the highly hygroscopic materials[19][20] |
| Mechanical Properties | ||
| Tensile strength (XY)MPa | >16.5 MPa printed XY, GB/T 1040; manufacturer lower bound, not an exact measurement.[1] | 38–51 (printed XY, ISO 527); Prusament 47 ± 2 at yield; 62 on My Tech Fun 4×4 mm bars[2][3][4][21] |
| Young's modulusMPa | Not documented | 1500–2311 (printed XY, ISO 527)[2][3][4][5] |
| Elongation at break% | >520% printed XY, GB/T 1040; manufacturer lower bound.[1] | 5.2–9.3 at break (printed XY, ISO 527); Prusament 5.1 at yield[3][4][5][2] |
| Flexural strengthMPa | Not documented | 58–80 (printed XY, ISO 178); Prusament 66 ± 2[2][3][4][5] |
| Flexural modulusMPa | Not documented | 1068–2277 (printed XY, ISO 178)[2][3][4][5] |
| Charpy impact, notchedkJ/m² | Not documented | 2.6 (PolyLite) to 11.6 (PolyMax) printed XY, ISO 179, notched; Prusament 6 ± 1[3][4][2] |
| Other impact data | Not documented | Charpy unnotched does not break on Prusa's 4 J pendulum (ISO 179-1); Izod 3.37 kJ/m² on My Tech Fun printed bars[2][21] |
| Layer adhesion / Z tensileMPa | 7.5 MPa printed Z, GB/T 1040 (manufacturer test)[1] | 18 ± 4 (Prusa interlayer adhesion test); 42.8 printed Z for PolyLite PETG; 33 on My Tech Fun bars[2][3][21] |
| Brittleness1–5 | Not documented | Moderate[2][3] |
| Hardness (scale-specific)Shore A / Shore D / Rockwell | 90 Shore A nominal grade designation; do not compare numerically with Shore D or Rockwell.[13] | 74 Shore D (Prusa Polymers method); measured on printed bars at 68.2 for Extrudr PETG, 72 for Fiberlogy PETG and 72.8 for Prusament PETG[2][21][22][23] |
| Creep resistance / sustained load1–5 | Not documented | Below average — a 12 mm bar sagged to 18.2 mm (Fiberlogy) and 19.4 mm (Bambu Lab Basic) over 5 days at 1.25 kg[21][15] |
| Fatigue / repeated-flex resistance1–5 | Not documented | Moderate — 79 000–193 000 cycles at 30 % of tensile strength, about three times printed PLA (R = 0.2, 7 Hz)[24] |
| Elasticity / flexibility1–5 | Not documented | Slightly flexible in thin sections[2] |
| Z strength as % of XY% | Not documented | 84 (PolyLite, printed Z against XY tensile)[3] |
| Thermal Properties | ||
| HDT at 0.45 MPa°C | Not documented | 68 (Prusament) to 78 (PolyLite), ISO 75 at 0.45 MPa[2][3][5] |
| HDT at 1.8 MPa°C | Not documented | 65 (Polymaker) to 75 (PolyLite), ISO 75 at 1.8 MPa; Prusament 68[2][3][5] |
| Glass transition (Tg)°C | Not documented | 71–81 (DSC)[3][4][5] |
| Melting point / Vicat°C | 110 °C Vicat softening (GB/T 1633, 120 °C/h, 10 N); not HDT or a continuous-use rating.[1] | Amorphous — no melting point; Vicat 75–84 (ISO 306)[3][4][5] |
| Continuous service temperature°C | Not documented | 61–66 — loaded bars begin to move at this temperature across six grades from four brands; Prusa publishes 68 for Prusament PETG[21][22][23][15][25] |
| Thermal expansion (CTE)µm/m·K | Not documented | 65 at 30 °C (neat PETG, large-format printed bead, TMA)[26] |
| Flammability / UL 94 | Not documented | Flammable; no UL 94 rating published for standard PETG, though flame-retardant V0 grades exist[27][20] |
| Environment & Chemical | ||
| UV resistance1–5 | Not documented | Moderate — a season or two[2] |
| Chemical resistance | Not documented | Withstands acids, alkalis, oils and UV exposure — Polymaker names outdoor use as a result[20] |
| Water / humidity resistance in service1–5 | Not documented | Good — minor absorption[2] |
| Food contact | Not documented | PET is the polymer of drinks bottles, but printed layer grooves harbour bacteria and no filament here carries a food-contact certification[20] |
| Biodegradability / compostability | Not documented | Not biodegradable[20] |
| Recyclability | Not documented | PET is widely recycled as bottle stock, but printed PETG waste is not accepted in household collection[20] |
| Health & Safety | ||
| Fume toxicity1–5 | Not documented | Moderate — measurable VOCs and UFPs, ventilation advised[28] |
| Ultrafine-particle emission rateparticles/min | Not documented | ≈5 × 10⁹ median for the PET-based T-Glase filament in the same chamber study, against ≈1 × 10⁸ for PLA[28] |
| Ventilation / filtration requirement1–5 | Not documented | Open a window / occasional ventilation[28] |
| Post-Processing | ||
| Sanding & machining | Not documented | Sands poorly — the material is tough and gums rather than powders[16] |
| Painting & finishing | Not documented | Paint adheres poorly without abrasion and a primer[2] |
| Gluing & solvent welding | Not documented | Cyanoacrylate; no common solvent welds PETG cleanly[16] |
| Vapour / chemical smoothing | Not documented | No practical vapour smoothing[2] |
| Support material pairing | Not documented | Prints its own supports; Polymaker rates PolyDissolve S1 for PETG[16] |
| Dimensional accuracy & detail | Not documented | Stringing and blobbing are the usual accuracy limits, not shrinkage[2][5] |
| Solvents & Solubility | ||
| Soluble in | Not documented | No common workshop solvent; 1,2-dichloroethane destroys it inside a week and dichloromethane — a carcinogen — dissolves the surface.[29][30] |
| Softened or crazed by | Not documented | Acetone (+16 % weight over 1 year at 23 °C), ethyl acetate, toluene and DMF swell and soften it; methanol crazes it.[29] |
| Solvent welding & smoothing agent | Not documented | Dichloromethane brushed on is the only agent that smooths PETG — a controlled carcinogen, not workshop stock.[30] |
Material entries describe families or representative grades, not an interchangeable specification for every spool. Test methods, orientations and conditions may differ. Unknown values are marked “Not documented”. Prices and source dates remain historical snapshots; check the linked guide for product details. Differences highlight text, not a universal winner.
Sources for this comparison
- eSUN PEBA-90A Technical Data Sheet v1.0 (Aug 2025), checked 2026-10-17 eSUN · 2025-08 · tds
- Prusament PETG Technical Datasheet v1.1 Prusa Polymers · 2022-02 · tds
- PolyLite PETG Technical Data Sheet Polymaker Wiki · 2026-08 · tds
- PolyMax PETG Technical Data Sheet Polymaker Wiki · 2026-08 · tds
- Polymaker PETG Technical Data Sheet Polymaker Wiki · 2026-08 · tds
- PETG Basic — product page Bambu Lab US Store · 2026-08 · vendor
- Polymaker product catalogue Polymaker · 2026-08 · vendor
- Printed Solid product catalogue Printed Solid · 2026-08 · vendor
- Black PETG Filament 1.75 mm 1 kg — product data Hatchbox · 2026-08 · vendor
- IEMAI PETG 3D Printing Filament product page IEMAI 3D · 2026-08 · vendor
- CHCKX PETG 3D Printer Filament 1.75 mm 1 kg, Black CHCKX (Amazon US) · 2026-08 · vendor
- ELEGOO product catalogue ELEGOO · 2026-08 · vendor
- eSUN PEBA-90A official product page: 1 kg price and product identity eSUN · 2026-10-17 · vendor
- Max volumetric speed Prusa Knowledge Base · 2026-08 · doc
- BambuLab PETG Basic vs Translucent vs PETG-CF — results spreadsheet My Tech Fun (Igor Gaspar) · 2026-08 · test
- PET and PETG — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- Filament Material Guide Prusa Knowledge Base · 2026-08 · doc
- Bambu Filament Technical Data Sheet — PETG HF Bambu Lab · 2026-08 · tds
- Wet Filament — signs, causes and drying Polymaker Wiki · 2026-08 · doc
- PETG — material basics Polymaker Wiki · 2026-08 · doc
- PCTG vs PETG comparison — results spreadsheet My Tech Fun (Igor Gaspar) · 2026-08 · test
- Extrudr PETG vs PCTG vs XPETG-CF — results spreadsheet My Tech Fun (Igor Gaspar) · 2026-08 · test
- Prusament PETG-CF vs PETG V0 vs PETG — results spreadsheet My Tech Fun (Igor Gaspar) · 2026-08 · test
- Mechanical Properties of Additively Manufactured Polymeric Materials — PLA and PETG — For Biomechanical Applications Polymers 16(13):1868 · 2024-06 · paper
- Prusament PETG — material page Prusa Polymers · 2026-08 · doc
- Effects of Fiber Orientation on the Coefficient of Thermal Expansion of Fiber-Filled Polymer Systems in Large Format Polymer Extrusion-Based Additive Manufacturing Materials 15(8):2764 · 2022-04 · paper
- Prusament PETG V0 Technical Datasheet Prusa Polymers · 2026-08 · tds
- Emissions of Ultrafine Particles and Volatile Organic Compounds from Commercially Available Desktop Three-Dimensional Printers with Multiple Filaments (Azimi et al.) Environmental Science & Technology 50(3) 1260-1268 · 2016-01 · paper
- Eastman Spectar copolyester — Chemical resistance (unstressed bars, 1 year at 23 °C) Eastman Chemical Company · 2026-08 · tds
- Improve your 3D prints with chemical smoothing Prusa Research · 2026-08 · doc