| Property | PC/ABS blendPC | High-Speed PLAPLA |
|---|---|---|
| Market snapshot | ||
| Listing priceUSD/kg; dated snapshots | $45.99/kg median; $34.99–$84.00/kg across 5 dated product listings | $19.99/kg median; $11.49–$32.99/kg across 10 dated product listings |
| Identity & Market | ||
| Base polymer / chemistry | Polycarbonate/ABS alloy — PC stiffness and heat resistance with ABS processability[1][2] | PLA with rheology and crystallisation tuned for high volumetric flow; melt index 15.4 g/10 min vs 7–11 for standard PLA[3][4] |
| Densityg/cm³ | 1.10 (Polymaker) and 1.24 (3DXTech FR grade), ISO 1183; Stratasys specific gravity 1.10 (ASTM D792)[1][2][5] | 1.23 (ISO 1183, at 21.5 °C)[3] |
| Typical priceUSD/kg | 1 kg spools cluster near 50[6][7] | Mainstream 1 kg spools cluster near 20[8][9][10] |
| Price range across brandsUSD/kg | 35–84 across brands; Reli3D 35, SUNLU 46, Polymaker 50, 3DXMAX 84[6][7][11][12] | 11–33 across brands; budget house brands 11–18, Prusament 33[13][14][15] |
| Market availability1–5 | Available from several mainstream brands[6][7] | Stocked by most mainstream brands[16][10][17] |
| Spool sizes & diameters | 1.75 and 2.85 mm; 0.5 and 1 kg spools[6][7] | 1.75 mm; 1 kg spools[8][10] |
| Typical applications | Automotive interior and electronics housings that need PC heat resistance without PC's warping[1] | Large or repetitive prints on printers that can sustain high flow[18][16] |
| Diameter tolerance± mm | Not documented | ±0.03 (Bambu Lab PLA Basic, rated to 258 mm/s)[19] |
| Printing Parameters | ||
| Nozzle temperature°C | 250–270 (Polymaker)[1] | 210–230 for high-speed work; 190–210 at classic speeds[3][16] |
| Bed temperature°C | 90–105 (Polymaker)[1] | 30–60 (Polymaker); 35–45 (Bambu Lab)[3][20] |
| Enclosure / chamber requirement1–5 | Enclosure required (passive) — Polymaker specifies a 90–100 °C chamber[1] | Open frame is fine[3] |
| Recommended chamber temperature°C | 90–100 (Polymaker)[1] | Not documented |
| Part cooling fan | Off (Polymaker)[1] | Fan on[3] |
| Bed surface & adhesion aid | PEI with a glue stick or a commercial adhesive[21] | Not documented |
| Maximum volumetric flow (mm³/s; see test conditions)mm³/s | 20 at Polymaker's 250 mm/s cap on a 0.4 mm nozzle at 0.2 mm layer[1][22] | ≈24 at 300 mm/s with a 0.4 mm nozzle and 0.2 mm layer; 30 % more flow than regular PLA at the same temperature[3][16][18][22] |
| Warping tendency1–5 | High — enclosure needed for reliable large parts[1][23] | None[3] |
| Bed-adhesion difficulty1–5 | Needs a specific surface plus adhesive[21][24] | Sticks to anything[25] |
| Stringing / oozing tendency1–5 | Moderate — retraction tuning needed; Polymaker flags stringing as a common PC problem[24] | Not documented |
| Overall printing difficulty1–5 | Advanced — enclosure, hardware upgrades, tuning[1][23] | Easy — minor profile tuning; needs a printer that can actually reach the flow rate[16][3] |
| Hardware Wear & Reliability | ||
| Nozzle hardness required1–4 | Brass fine indefinitely[23] | Brass fine indefinitely[26] |
| Abrasiveness1–5 | Non-abrasive[1] | Non-abrasive[27][26] |
| Nozzle clog risk1–5 | Moderate — needs dry filament and a clean nozzle; 3DXTech lists no special nozzle concerns but a 120 °C pre-dry of 4 h or more[28] | Very low[26] |
| Heat-creep / jam sensitivity1–5 | Slightly sensitive[21] | Moderate — good heatbreak cooling needed; PLA softens below 60 °C[29] |
| Hotend requirement | All-metal hot end required (Simplify3D)[21] | No special hot-end required[25] |
| Moisture Behaviour | ||
| Moisture absorption (hygroscopicity)1–5 | Low (0.1–0.3 %) — the PC matrix takes up 0.15–0.25 % and 3DXTech specifies a 120 °C, 4 h or more pre-dry[30][31][28] | Moderate — 0.40 % equilibrium at 23 °C / 70 % RH[3] |
| Equilibrium moisture content at ~50 % RH% | Not documented | 0.40 equilibrium at 23 °C / 70 % RH (Polymaker PolySonic)[3] |
| Drying temperature & time | 75 °C for 6 h (Polymaker)[1] | 55 °C for 6 h; 50 °C for 8 h (Bambu Lab)[3][20] |
| Symptoms when wet | Bubbling and popping at the nozzle, stringing and a rough surface[32] | Bubbling and popping at the nozzle, stringing, rough surface and weak layers[32] |
| Effect of moisture on strength | No dry-versus-conditioned figures are published. Polymaker calls PC highly hygroscopic and requires a 70–80 °C dry for 6–8 h; run wet, the loss shows as surface defects and poor layer adhesion[24][32] | Polymaker rates PLA low-sensitivity — the loss shows as poor layer adhesion and brittle layers rather than a published strength figure[32] |
| Storage requirement | Airtight containers with desiccant to prevent reabsorption[24] | Sealed with desiccant below 20 % RH; shelf life at ambient is long[20][25] |
| Mechanical Properties | ||
| Tensile strength (XY)MPa | 39.9 ± 1.0 printed XY, ISO 527 (Polymaker); 3DXTech quotes 60 at break for its FR PC/ABS[1][2] | 43.9 at 300 mm/s and 46.0 at 46.7 mm/s (printed XY, ISO 527); 58.6 on My Tech Fun bars for Creality Hyper PLA[3][33] |
| Young's modulusMPa | 1835 ± 65 printed XY, ISO 527 (Polymaker); 3DXTech quotes 2250[1][2] | 2650 at 300 mm/s, 2878 at classic speed (printed XY, ISO 527)[3] |
| Elongation at break% | 4.2 ± 0.3 printed XY, ISO 527 (Polymaker); 3DXTech quotes 10 at break[1][2] | 15.1 at 300 mm/s, 21.5 at classic speed (printed XY, ISO 527)[3] |
| Flexural strengthMPa | 66.3 ± 0.9 printed XY, ISO 178 (Polymaker); 3DXTech quotes 85[1][2] | 71.4 at 300 mm/s, 76.5 at classic speed (printed XY, ISO 178)[3] |
| Flexural modulusMPa | 2081 ± 106 printed XY, ISO 178 (Polymaker); 3DXTech quotes 2300[1][2] | 2798 at 300 mm/s, 2868 at classic speed (printed XY, ISO 178)[3] |
| Charpy impact, notchedkJ/m² | 25.8 ± 1.3 printed XY, ISO 179, notched (Polymaker) — above both unfilled PC and ABS[1] | 5.0 at 300 mm/s, 6.1 at classic speed (printed XY, ISO 179, notched)[3] |
| Other impact data | Notched Charpy still 13 ± 2 kJ/m² at −30 °C printed XY (Polymaker, ISO 179-1/1eA), against 1.5 in Z. Stratasys prints Izod notched at 241 J/m XZ against 34.0 J/m ZX, and unnotched 655 against 101 J/m (ASTM D256, F900 T16).[1][5] | Printing at 300 mm/s instead of 46.7 mm/s costs 4.6 % tensile strength and 18 % notched Charpy[3] |
| Layer adhesion / Z tensileMPa | 25.9-30.2 at break printed ZX (Stratasys, ASTM D638 on the F900 and Fortus 450mc); 22.9 +/- 1.2 printed Z, ISO 527 (Polymaker)[1][5] | 32.4 at 300 mm/s, 37.3 at classic speed (printed Z, ISO 527); 35.3 for Creality Hyper PLA vs 23.0 for average PLA on identical bars[3][33] |
| Brittleness1–5 | Tough — absorbs impact, yields before breaking[1] | Moderate[3] |
| Hardness (scale-specific)Shore A / Shore D / Rockwell | Rockwell 70 (118) — the source does not name the scales and Shore D 79 on extruded unfilled PC stock (ASTM D785, D2240); no figure is published for a PC/ABS filament[34] | 78.7 Shore D measured on printed bars for Sunlu PLA Meta (My Tech Fun), against 75.3 for the same maker's plain PLA[35] |
| Creep resistance / sustained load1–5 | Good. Room-temperature tensile creep of moulded PC/ABS was still running unbroken at 30 MPa when the experiment was stopped for time; specimens failed within the test window at 39-47 MPa (ASTM D638)[36] | Poor — 12 mm bar sagged to 17.7 mm over 6 days at 1.25 kg[33] |
| Fatigue / repeated-flex resistance1–5 | Not documented | Poor — no grade-specific S-N curve; plain printed PLA ran 38 000–49 000 cycles at 30 % of tensile strength (R = 0.2)[37][29] |
| Elasticity / flexibility1–5 | Rigid[1] | Rigid[3] |
| Z strength as % of XY% | 75-86 (Stratasys ZX against XZ tensile at break, ASTM D638) against 57 (Polymaker, printed Z against XY tensile)[1][5] | 74 at 300 mm/s, 81 at classic speed (printed)[3] |
| Thermal Properties | ||
| HDT at 0.45 MPa°C | 112 (ISO 75 at 0.45 MPa, Polymaker); Stratasys prints 117.9 in XY and 126.1 in XZ (ASTM D648 Method B at 66 psi), against 125.0 moulded[1][5] | 53 (ISO 75, 0.45 MPa)[3] |
| HDT at 1.8 MPa°C | 106 (ISO 75 at 1.8 MPa, Polymaker); Stratasys prints 107.5 in XY and 112.0 in XZ (ASTM D648 Method B at 264 psi), against 102.9 moulded[1][5] | 52 (ISO 75, 1.8 MPa)[3] |
| Glass transition (Tg)°C | 109 (Polymaker) and 137 (3DXTech FR grade), DSC; Stratasys measures 105.3 (ASTM D7426 inflection point)[1][2][5] | 59 (DSC)[3] |
| Melting point / Vicat°C | Amorphous — no melting point; Vicat 135 (Polymaker, ISO 306)[1] | 164 peak melt (DSC); crystallisation 96 °C, Vicat 61 °C[3] |
| Continuous service temperature°C | 113 — Prusa publishes this as the temperature resistance of Prusament PC Blend[31] | 53 — loaded bars begin to move at this temperature[33] |
| Annealing response | 90 °C for 2 h (Polymaker)[1] | Not documented |
| Thermal expansion (CTE)µm/m·K | 59.9 over -50 to 35 °C and 73.0 over -50 to 95 °C (printed XY, ASTM E831)[5] | 96–99 for plain printed PLA (fibre Bragg grating, 25–50 °C); no grade-specific measurement published[38] |
| Flammability / UL 94 | Not documented | Flammable; no UL 94 rating published by the major brands[20][4] |
| Environment & Chemical | ||
| UV resistance1–5 | Degrades within weeks outdoors[24] | Degrades within weeks outdoors[29][39] |
| Chemical resistance | Withstands oils, solvents and fuels; Polymaker rates it good against weak acids[24] | Good against weak acids, oils and grease; poor against strong acids and alkalis[3] |
| Water / humidity resistance in service1–5 | Not documented | Good — insoluble in water[20] |
| Food contact | Bisphenol-A polycarbonate is not offered as food-contact filament[24] | Base resin is food-contact grade, but printed layer grooves harbour bacteria; Prusa advises against food use[29] |
| Biodegradability / compostability | Not biodegradable[24] | Industrially compostable only — needs sustained 55 °C; not home compostable[40][29] |
| Recyclability | Mechanically recyclable but not accepted in household plastic collection[24] | Mechanically recyclable; not accepted in household plastic collection[40] |
| Health & Safety | ||
| Fume toxicity1–5 | Moderate — measurable VOCs and UFPs, ventilation advised[41] | Low hazard — minimal VOC and particle emission[41] |
| Ultrafine-particle emission rateparticles/min | ≈4 × 10¹⁰ median — the highest ultrafine-particle rate of the nine filaments in the chamber study, above every ABS tested[41] | Not documented |
| Ventilation / filtration requirement1–5 | Ventilated room or enclosure recommended[41][23] | None needed in a normal room[41] |
| Post-Processing | ||
| Sanding & machining | Sands and machines well; the toughness means it cuts rather than chips[21] | Wet sanding — dry sanding heats the surface by friction and smears it[39][29] |
| Gluing & solvent welding | Cyanoacrylate; dichloromethane solvent-welds PC but is a laboratory reagent[21] | Cyanoacrylate for most joints; some grades partially dissolve and bond with acetone[29][42] |
| Vapour / chemical smoothing | Acetone attacks the ABS phase, so surface smoothing is partial rather than full[1] | No practical vapour smoothing — only chloroform, hot benzene or THF, which are laboratory-only[29] |
| Support material pairing | Prints its own supports; 3DXTech sells a dedicated PC break-away support[21] | PolySupport and PolyDissolve S1 (Polymaker)[3] |
| Solvents & Solubility | ||
| Soluble in | Dichloromethane and chloroform dissolve the PC phase; acetone, MEK and THF dissolve the ABS phase.[43][44] | Chloroform: 10 % w/v in 2–4 h at 23 °C, every grade and morphology; THF and DMF only at 65 °C. Laboratory reagents.[45] |
| Softened or crazed by | Petrol, esters, ether and 1 % alkali stress-crack the PC phase; aromatics and esters soften the ABS phase.[43][44] | Acetone, ethyl acetate and toluene plasticise it but dissolve <1 % even at 65 °C; submersion in acetone crazes and destroys parts.[45][46] |
| Solvent welding & smoothing agent | Acetone attacks only the ABS phase, so smoothing is partial; a dichloromethane cement welds the whole section.[1][47] | Chloroform vapour smooths and welds PLA at the cost of tensile strength; acetone does not smooth it at all.[48][46] |
Material entries describe families or representative grades, not an interchangeable specification for every spool. Test methods, orientations and conditions may differ. Unknown values are marked “Not documented”. Prices and source dates remain historical snapshots; check the linked guide for product details. Differences highlight text, not a universal winner.
Sources for this comparison
- Polymaker PC-ABS Technical Data Sheet V5.4 Polymaker · 2024-11 · tds
- Firewire Flame Retardant PC/ABS Technical Data Sheet Rev 3.0 3DXTech · 2026-08 · tds
- PolySonic PLA Technical Data Sheet V5.4 Polymaker · 2024-11 · tds
- PolyLite PLA Technical Data Sheet V5.4 Polymaker · 2024-11 · tds
- PC-ABS — FDM Material Data Sheet Stratasys · 2023-08 · tds
- Polymaker product catalogue Polymaker · 2026-08 · vendor
- 3DXTech product catalogue 3DXTech · 2026-08 · vendor
- PolySonic PLA 1.75mm/1kg — product page Polymaker Shop · 2026-08 · vendor
- Overture High Speed PLA 1.75mm Overture3D · 2026-08 · vendor
- High Speed PLA filament collection Anycubic Official Store · 2026-08 · vendor
- Reli3D PC-ABS Filament, Black, 1000 g spool Reli3D (Amazon US) · 2026-08 · vendor
- SUNLU PC-ABS 3D Printer Filament 1 kg SUNLU · 2026-08 · vendor
- PLA Meta filament collection Sunlu Official Store · 2026-08 · vendor
- QIDI PLA Rapido 1.75mm 1kg 3D Printers Depot · 2026-08 · vendor
- Prusament PLA Prusa Pro Green 1kg (NFC) Prusa Research · 2026-08 · vendor
- PolySonic PLA — product page Polymaker · 2026-08 · vendor
- Creality PLA filament collection Creality Official Store · 2026-08 · vendor
- Polymaker Launches New High-Speed 3D Printing Filament — PolySonic PLA & PLA Pro Polymaker · 2023-11 · doc
- PLA Basic — product page Bambu Lab US Store · 2026-08 · vendor
- Bambu Filament Technical Data Sheet V3.0 — PLA Basic Bambu Lab · 2026-08 · tds
- Polycarbonate — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- Max volumetric speed Prusa Knowledge Base · 2026-08 · doc
- ABS / ASA / PC Usage Guide Bambu Lab Wiki · 2026-08 · doc
- PC — material basics Polymaker Wiki · 2026-08 · doc
- PLA — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- Filament Material Guide Prusa Knowledge Base · 2026-08 · doc
- Prusament PLA — material page Prusa Polymers · 2026-08 · doc
- 3DXTech 3DXMAX ABS product page 3DXTech · 2026-08 · vendor
- PLA — material guide Prusa Knowledge Base · 2026-08 · doc
- Bambu Filament Technical Data Sheet V2.0 — PC Bambu Lab · 2026-08 · tds
- Prusament PC Blend Technical Datasheet v1.1 Prusa Polymers · 2022-02 · tds
- Wet Filament — signs, causes and drying Polymaker Wiki · 2026-08 · doc
- Creality Hyper PLA filament review — results spreadsheet My Tech Fun (Igor Gaspar) · 2026-08 · test
- TECANAT natural (PC) — stock shape properties Ensinger · 2026-08 · tds
- Carbon Fiber PLA vs META-PLA vs PLA+ vs PLA by Sunlu — results spreadsheet My Tech Fun (Igor Gaspar) · 2026-08 · test
- Experimental data for creep and dynamic mechanical properties of polycarbonate and polycarbonate/ABS Data in Brief 42:108264 · 2022-06 · paper
- Mechanical Properties of Additively Manufactured Polymeric Materials — PLA and PETG — For Biomechanical Applications Polymers 16(13):1868 · 2024-06 · paper
- Characterization of Thermal Expansion Coefficient of 3D Printing Polymeric Materials Using Fiber Bragg Grating Sensors Materials 17(18):4668 · 2024-09 · paper
- Prusament PLA Technical Data Sheet v1.0 Prusa Polymers · 2018-09 · tds
- Filamentive PLA (recycled) — product page Filamentive · 2026-08 · vendor
- Emissions of Ultrafine Particles and Volatile Organic Compounds from Commercially Available Desktop Three-Dimensional Printers with Multiple Filaments (Azimi et al.) Environmental Science & Technology 50(3) 1260-1268 · 2016-01 · paper
- Prusament rPLA Corn Pigment 1kg — product page Prusa Research · 2026-08 · vendor
- Makrolon — The chemical resistance (Makrolon 2800, 6 days at 23 °C and 50 °C) Covestro · 2016-12 · tds
- Chemical resistance — resistance of Ensinger plastics to chemicals (DIN 50 014, 23/50) Ensinger · 2026-08 · tds
- Solubility Study of Ingeo Biopolymer Grades in Common Organic Solvents (NWPD003) NatureWorks · 2019-10 · tds
- Improve your 3D prints with chemical smoothing Prusa Research · 2026-08 · doc
- Weld-On 3 Acrylic Plastic Cement — technical data sheet (shipped as dichloromethane) IPS Corporation · 2002-07 · tds
- Effect of vapour smoothing in trichloromethane on 3D printed PLA — surface, mechanical and chemical structure Pitale, Keche & Chopra, Engineering Research Express 6(4) 045579 · 2024-12 · paper