Filament comparison
ASA-CF vs PC-ESD
Compare printing settings, strength, heat resistance, dated prices and sources.
2 selected · all documented properties
| Property | Carbon-fibre ASA (ASA-CF)ASA | ESD-safe PCPC |
|---|---|---|
| Market snapshot | ||
| Listing priceUSD/kg; dated snapshots | $36.99/kg median; $25.00–$90.00/kg across 5 dated product listings | $180.00/kg median; $180.00–$180.00/kg across 1 dated product listings |
| Identity & Market | ||
| Base polymer / chemistry | ASA reinforced with chopped carbon fibre — Formfutura's ApolloX CF10 is 10 wt%[1][2][3] | Polycarbonate compounded with a conductive filler for static-dissipative parts[4] |
| Densityg/cm³ | 1.02 (Bambu Lab), 1.1 (Formfutura ApolloX CF10) and 1.11 (3DXTech), ISO 1183[1][2][3] | 1.24 (ISO 1183, 3DXTech); Stratasys specific gravity 1.195 (ASTM D792)[4][5] |
| Typical priceUSD/kg | 1 kg spools cluster near 37[6][7] | 1 kg-equivalent spools cluster near 180[8] |
| Price range across brandsUSD/kg | 25–90 across brands; IEMAI 25, Ambrosia 33, Bambu Lab 37, Polymaker Fiberon 40, 3DXTech 90[9][6][7][8][10] | 180 at 3DXTech's 750 g pricing — the most expensive material in this group[8] |
| Market availability1–5 | Available from several mainstream brands[6][7][8][9] | Special order, 1–2 makers worldwide[8] |
| Spool sizes & diameters | 1.75 and 2.85 mm; 0.5, 0.75 and 1 kg spools[7][8][6] | 1.75 and 2.85 mm; 750 g spools plus Stratasys-compatible cartridges[8] |
| Typical applications | Outdoor structural parts, drone and antenna mounts where stiffness and UV stability both matter[1][2] | Electronics fixtures and trays that need PC heat resistance and static dissipation together[4] |
| Printing Parameters | ||
| Nozzle temperature°C | 250–280 (Bambu Lab)[1] | Not documented |
| Bed temperature°C | 80–100 (Bambu Lab)[1] | Not documented |
| Enclosure / chamber requirement1–5 | Enclosure recommended — Bambu Lab specifies a 45–60 °C chamber[1][11] | Enclosure required (passive)[11][12] |
| Recommended chamber temperature°C | 45–60 (Bambu Lab)[1] | Not documented |
| Part cooling fan | Fan on (Bambu Lab)[1] | Not documented |
| Bed surface & adhesion aid | PEI sheet, BuildTak or an adhesion aid such as Magigoo (Polymaker); Simplify3D also lists Kapton tape and ASA slurry[13][14] | PEI with a glue stick or a commercial adhesive[15] |
| Maximum volumetric flow (mm³/s; see test conditions)mm³/s | 20 at Bambu Lab's 250 mm/s cap on a 0.4 mm nozzle at 0.2 mm layer[1][16] | Not documented |
| Warping tendency1–5 | Moderate — needs adhesion aid or draught shield; the fibre reduces warping against unfilled ASA[11] | Severe — heated chamber needed[11][12] |
| Bed-adhesion difficulty1–5 | Needs a specific surface plus adhesive[13] | Needs a specific surface plus adhesive[15][17] |
| Stringing / oozing tendency1–5 | Slight — Polymaker advises 1–2 mm retraction at 20–30 mm/s[13] | Moderate — retraction tuning needed; Polymaker flags stringing as a common PC problem[17] |
| Overall printing difficulty1–5 | Intermediate — dry filament and a tuned profile; hardened nozzle mandatory[11] | Advanced — enclosure, hardware upgrades, tuning[11] |
| Hardware Wear & Reliability | ||
| Nozzle hardness required1–4 | Hardened steel required[11] | Hardened steel required[4] |
| Abrasiveness1–5 | Highly abrasive — standard CF composite[11] | Moderately abrasive — conductive carbon filler[4] |
| Nozzle clog risk1–5 | Moderate — needs dry filament and a clean nozzle; Prusa lists higher risk of nozzle clogging for fibre-filled composites and Simplify3D a higher tendency to clog[18][19] | Moderate — needs dry filament and a clean nozzle; 3DXTech lists no special nozzle concerns but a 120 °C pre-dry[20] |
| Heat-creep / jam sensitivity1–5 | Slightly sensitive[14] | Slightly sensitive[15] |
| Hotend requirement | No special hotend required[14] | All-metal hot end required (Simplify3D)[15] |
| Moisture Behaviour | ||
| Moisture absorption (hygroscopicity)1–5 | Moderate — 0.33 % saturated at 25 °C / 55 % RH (Bambu Lab)[1] | Low (0.1–0.3 %) — the PC matrix takes up 0.15–0.25 % and 3DXTech specifies a 120 °C, 4 h pre-dry[21][22][20] |
| Equilibrium moisture content at ~50 % RH% | 0.33 saturated at 25 °C / 55 % RH (Bambu Lab)[1] | Not documented |
| Drying temperature & time | 80 °C for 8 h (Bambu Lab)[1] | Not documented |
| Symptoms when wet | Bubbling and popping at the nozzle, stringing and a rough surface[23] | Bubbling and popping at the nozzle, stringing and a rough surface[23] |
| Effect of moisture on strength | No dry-versus-conditioned figures are published; Polymaker groups the styrenics as moderate-sensitivity and absorbed water shows as bubbling and poor layer adhesion[23] | No dry-versus-conditioned figures are published. Polymaker calls PC highly hygroscopic and requires a 70–80 °C dry for 6–8 h; run wet, the loss shows as surface defects and poor layer adhesion[17][23] |
| Storage requirement | Sealed with desiccant; Polymaker rates the styrenics moderate-sensitivity[23] | Airtight containers with desiccant to prevent reabsorption[17] |
| Mechanical Properties | ||
| Tensile strength (XY)MPa | 34 ± 3 printed XY, ISO 527 (Bambu Lab); 3DXTech quotes 48 at break and Formfutura 79 at 23 °C[1][2][3] | 68 at break (printed XY, ISO 527, 3DXTech) — above the 58 of 3DXTech's unfilled ezPC; Stratasys prints 47.6-49.4 at yield in XZ (ASTM D638)[4][24][5] |
| Young's modulusMPa | 4200 ± 270 printed XY, ISO 527 (Bambu Lab); 3DXTech quotes 5355 and Formfutura 7580[1][2][3] | 2300 (printed XY, ISO 527); Stratasys prints 1960 in XZ and 1810-1910 in ZX (ASTM D638)[4][5] |
| Elongation at break% | 9.6 ± 1.4 printed XY, ISO 527 (Bambu Lab); 3DXTech quotes 3 at break and Formfutura 1.8[1][2][3] | 6 at break (printed XY, ISO 527), against 14 for the unfilled grade[4][24] |
| Flexural strengthMPa | 72 ± 5 printed XY, ISO 178 (Bambu Lab); 3DXTech quotes 78[1][2] | 95 (printed XY, ISO 178); Stratasys prints 82.6-83.2 at break in XZ against 46.3-49.5 in ZX (ASTM D790)[4][5] |
| Flexural modulusMPa | 3740 ± 130 printed XY, ISO 178 (Bambu Lab); 3DXTech quotes 5210[1][2] | 2310 (printed XY, ISO 178)[4] |
| Charpy impact, notchedkJ/m² | 6.2 ± 1.4 printed XY, ISO 179, notched (Bambu Lab) — a third of unfilled Bambu Lab ASA's 19.6[1][25] | Not documented |
| Other impact data | Charpy unnotched 14.0 ± 2.2 printed XY (Bambu Lab, ISO 179), against 41.0 for unfilled Bambu Lab ASA[1][25] | Not documented |
| Layer adhesion / Z tensileMPa | 30 ± 4 printed Z, ISO 527 (Bambu Lab); flexural Z falls to 33 against 72 in XY[1] | 32.5-37.9 at yield printed ZX (Stratasys, ASTM D638 on the Fortus 450mc and F900)[5] |
| Brittleness1–5 | Brittle — snaps with little warning[1][2] | Moderate[4] |
| Hardness (scale-specific)Shore A / Shore D / Rockwell | Not documented | Rockwell 70 (118) — the source does not name the scales and Shore D 79 on extruded unfilled PC stock (ASTM D785, D2240); no figure is published for an ESD grade[26] |
| Creep resistance / sustained load1–5 | Good — no creep test found; chopped carbon fibre lifts modulus to 4200 MPa against 2379–2450 for unfilled ASA[1][27] | Excellent — holds load for years. Moulded unfilled PC was still running unbroken under 41 MPa tensile creep at room temperature when the test was stopped, and the conductive filler leaves the glass transition unchanged at 142 °C, so the creep mechanism is polycarbonate's[28][5] |
| Fatigue / repeated-flex resistance1–5 | Below average — no CF-grade S-N curve; notched Charpy falls to 6.2 kJ/m² against 19.6 for unfilled Bambu Lab ASA[1][25] | Not documented |
| Elasticity / flexibility1–5 | Rigid[1] | Rigid[4] |
| Z strength as % of XY% | 88 by tensile, 46 by flexural (printed, Bambu Lab)[1] | 68-77 (Stratasys ZX against XZ tensile yield, ASTM D638)[5] |
| Thermal Properties | ||
| HDT at 0.45 MPa°C | 110 (ISO 75, 0.45 MPa, Bambu Lab) against 100 for unfilled Bambu Lab ASA[1][25] | 143-146 printed in XY, XZ and ZX (Stratasys, ASTM D648 Method B at 66 psi); 135 moulded[5] |
| HDT at 1.8 MPa°C | 102 (ISO 75, 1.8 MPa, Bambu Lab) against 92 for unfilled Bambu Lab ASA[1][25] | 140-144 printed in XY, XZ and ZX (Stratasys, ASTM D648 Method B at 264 psi); 124 moulded[5] |
| Glass transition (Tg)°C | Not documented | 143 (DSC, 3DXTech) and 142 (Stratasys, ASTM D7426)[4][5] |
| Continuous service temperature°C | 93 — Prusa publishes this as the temperature resistance of Prusament ASA[29] | 113 — Prusa publishes this as the temperature resistance of Prusament PC Blend[22] |
| Thermal expansion (CTE)µm/m·K | Not documented | 68.4 on extruded unfilled PC stock (ASTM D696; source states 3.8e-5 in/in/°F); no figure is published for a conductive-filled grade[26] |
| Flammability / UL 94 | Flammable; no UL 94 rating published[25] | Not documented |
| Environment & Chemical | ||
| UV resistance1–5 | Excellent — designed for permanent outdoor use; the acrylate rubber phase is unchanged by the fibre[30][13] | Not documented |
| Chemical resistance | Good against weak acids, weak alkalis, oils and grease; dissolved by acetone[27] | Withstands oils, solvents and fuels; Polymaker rates it good against weak acids[17] |
| Food contact | Not food safe[13] | Bisphenol-A polycarbonate is not offered as food-contact filament[17] |
| Biodegradability / compostability | Not biodegradable[13] | Not biodegradable[17] |
| Recyclability | Not accepted in household plastic collection[13] | Mechanically recyclable but not accepted in household plastic collection[17] |
| Electrical & ESD properties | Surface resistance above 10⁹ ohm/sq — not static-dissipative (3DXTech, ASTM D257)[2] | Surface resistance 10⁷–10⁹ ohm/sq, the static-dissipative band (ASTM D257), against above 10¹³ for unfilled ezPC[4][24] |
| Health & Safety | ||
| Fume toxicity1–5 | High — hazardous VOC such as styrene; enclosure and filtration needed[31][11] | Moderate — measurable VOCs and UFPs, ventilation advised[31] |
| Ultrafine-particle emission rateparticles/min | Not documented | ≈4 × 10¹⁰ median — the highest ultrafine-particle rate of the nine filaments in the chamber study, above every ABS tested[31] |
| Hazardous species emitted | Styrene. Bambu Lab states ABS and ASA release harmful gases such as styrene at printing temperature, which can be toxic and cause dizziness or nausea. Azimi et al. measured styrene from every styrenic filament tested but did not test ASA itself[11][31] | Not documented |
| Ventilation / filtration requirement1–5 | Enclosure with carbon and HEPA filtration[31][11] | Ventilated room or enclosure recommended[31][11] |
| Dust & fibre handling hazard | Carbon fibre is bound in the matrix; sanding dust should not be inhaled[2] | Conductive carbon filler is bound in the matrix; avoid inhaling sanding dust[4] |
| Post-Processing | ||
| Sanding & machining | Sands well and takes filler before painting[13] | Sands and machines well; the toughness means it cuts rather than chips[15] |
| Painting & finishing | Paints readily; ASA holds colour outdoors so many parts are left unpainted[13] | Not documented |
| Gluing & solvent welding | Solvent-welds with acetone[27] | Cyanoacrylate; dichloromethane solvent-welds PC but is a laboratory reagent[15] |
| Vapour / chemical smoothing | Acetone vapour smoothing works[27] | No practical vapour smoothing[15] |
| Support material pairing | HIPS breaks away or dissolves in d-limonene; Bambu Lab sells a Support for ABS that also serves ASA[11] | Prints its own supports; 3DXTech sells a dedicated PC break-away support[15] |
| Dimensional accuracy & detail | Matte fibre-filled finish hides layer lines[1] | Not documented |
| Solvents & Solubility | ||
| Soluble in | Acetone dissolves the resin and leaves the fibre; MEK, THF, ethyl acetate and chlorinated solvents attack the styrenic backbone.[32][27] | Dichloromethane, chloroform, DMF and dioxane dissolve it outright (Covestro, 6 days at 23 °C). Laboratory reagents.[33] |
| Softened or crazed by | Limonene attacks some grades — Prusa reports Prusament ASA Orange flaking apart as layer adhesion fails.[34] | Methanol, butyl acetate, ether, 1 % NaOH and phthalate plasticisers stress-crack it; acetone, MEK and xylene swell it.[33] |
| Solvent welding & smoothing agent | Acetone vapour reaches only the resin fraction, so the fibre is left standing proud of the smoothed surface.[35][27] | Dichloromethane cement welds PC — 16.5 MPa lap shear at one week (IPS Weld-On 3). A controlled carcinogen.[36] |
Material entries describe families or representative grades, not an interchangeable specification for every spool. Test methods, orientations and conditions may differ. Unknown values are marked “Not documented”. Prices and source dates remain historical snapshots; check the linked guide for product details. Differences highlight text, not a universal winner.
Sources for this comparison
- Bambu Filament Technical Data Sheet V1.0 — ASA-CF Bambu Lab · 2026-08 · tds
- CarbonX Carbon Fiber ASA Technical Data Sheet 3DXTech · 2026-08 · tds
- ApolloX CF10 Technical Data Sheet Formfutura · 2026-08 · tds
- 3DXSTAT ESD-PC Technical Data Sheet 3DXTech · 2026-08 · tds
- PC-ESD — FDM Material Data Sheet Stratasys · 2024-10 · tds
- ASA-CF — product page Bambu Lab US Store · 2026-08 · vendor
- Polymaker product catalogue Polymaker · 2026-08 · vendor
- 3DXTech product catalogue 3DXTech · 2026-08 · vendor
- Filastruder product catalogue Filastruder · 2026-08 · vendor
- IEMAI CF-ASA 3D Printing Filament product page IEMAI 3D · 2026-08 · vendor
- ABS / ASA / PC Usage Guide Bambu Lab Wiki · 2026-08 · doc
- PolyLite PC Technical Data Sheet V5.4 Polymaker · 2024-11 · tds
- ASA — material basics Polymaker Wiki · 2026-08 · doc
- ASA — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- Polycarbonate — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- Max volumetric speed Prusa Knowledge Base · 2026-08 · doc
- PC — material basics Polymaker Wiki · 2026-08 · doc
- Composite materials filled with carbon, kevlar or glass Prusa Knowledge Base · 2026-08 · doc
- Carbon Fiber Filled — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- 3DXSTAT ESD-PC — product page (print recommendations) 3DXTech · 2026-08 · doc
- Bambu Filament Technical Data Sheet V2.0 — PC Bambu Lab · 2026-08 · tds
- Prusament PC Blend Technical Datasheet v1.1 Prusa Polymers · 2022-02 · tds
- Wet Filament — signs, causes and drying Polymaker Wiki · 2026-08 · doc
- ezPC Polycarbonate Technical Data Sheet 3DXTech · 2026-08 · tds
- Bambu Filament Technical Data Sheet V3.0 — ASA Bambu Lab · 2026-08 · tds
- TECANAT natural (PC) — stock shape properties Ensinger · 2026-08 · tds
- PolyLite ASA Technical Data Sheet Polymaker · 2024-11 · tds
- Experimental data for creep and dynamic mechanical properties of polycarbonate and polycarbonate/ABS Data in Brief 42:108264 · 2022-06 · paper
- Prusament ASA — material page Prusa Polymers · 2026-08 · doc
- ASA — FDM Material Data Sheet (includes 1000 h QUV exposure results) Stratasys · 2026-08 · tds
- Emissions of Ultrafine Particles and Volatile Organic Compounds from Commercially Available Desktop Three-Dimensional Printers with Multiple Filaments (Azimi et al.) Environmental Science & Technology 50(3) 1260-1268 · 2016-01 · paper
- Chemical resistance — resistance of Ensinger plastics to chemicals (DIN 50 014, 23/50) Ensinger · 2026-08 · tds
- Makrolon — The chemical resistance (Makrolon 2800, 6 days at 23 °C and 50 °C) Covestro · 2016-12 · tds
- HIPS — Knowledge Base Prusa Research · 2026-08 · doc
- Improve your 3D prints with chemical smoothing Prusa Research · 2026-08 · doc
- Weld-On 3 Acrylic Plastic Cement — technical data sheet (shipped as dichloromethane) IPS Corporation · 2002-07 · tds