Filament comparison
ABS vs POM
Compare printing settings, strength, heat resistance, dated prices and sources.
2 selected · all documented properties
| Property | ABSABS | POM (acetal)ENGINEERING |
|---|---|---|
| Market snapshot | ||
| Listing priceUSD/kg; dated snapshots | $19.99/kg median; $11.99–$45.00/kg across 16 dated product listings | Not documented |
| Identity & Market | ||
| Base polymer / chemistry | Acrylonitrile butadiene styrene — a styrenic terpolymer with a butadiene rubber phase[1][2] | Polyoxymethylene, normally the copolymer POM-C. Apium's filament grade is POM-C with antistatic additives; no unfilled POM filament was found on sale[3][4] |
| Densityg/cm³ | 1.04 (Polymaker PolyLite ABS and ABS Pro) to 1.06 (ABS Max), ISO 1183; Bambu Lab 1.05[5][1][6][7] | 1.41 (extruded POM-C stock)[3] |
| Typical priceUSD/kg | 1 kg spools cluster near 20[8][9][10][11][12] | Not documented |
| Price range across brandsUSD/kg | 12–45 across brands; IEMAI 12, SUNLU 12 at a 3 kg minimum, ELEGOO 15 in a 5 kg pack, Polymaker 19, YXPOLYER 20, Bambu Lab 20, Push Plastic 25, 3DXTech 45[8][9][13][14][10][11][12][15] | Not documented |
| Market availability1–5 | Ubiquitous, every brand and retailer[8][9][13][14] | Special order, 1-2 makers worldwide — Apium sells a POM-C ESD filament through its own shop and states its printers are the only ones able to process POM-C; no POM filament appears in the 3DJAKE or igo3d product sitemaps, at MatterHackers or at Printed Solid[4][16][17][18] |
| Spool sizes & diameters | 1.75 and 2.85 mm; 1, 5 and 10 kg spools[13][14] | Not documented |
| Typical applications | Enclosures, automotive interior parts and tooling that must hold shape above PLA's 55 °C ceiling[1][19] | Gears, bushings, bearings, conveyor and food-machinery parts; Apium markets its POM-C ESD grade for semiconductor insulators, aerospace fasteners and sliding parts[3][4] |
| Printing Parameters | ||
| Nozzle temperature°C | 240–270 (Bambu Lab); 245–265 (Polymaker PolyLite)[5][1] | Not documented |
| Bed temperature°C | 80–100 (Bambu Lab); 90–100 (Polymaker)[5][1] | Not documented |
| Enclosure / chamber requirement1–5 | Enclosure recommended — Polymaker calls a chamber needed at ambient temperature, Bambu Lab requires an enclosed printer and rules out its P1P and A-series machines[1][20] | Not documented |
| Recommended chamber temperature°C | 45–60 (Bambu Lab)[5] | Not documented |
| Part cooling fan | 0–80 % (Bambu Lab); off (Polymaker PolyLite)[5][1] | Not documented |
| Bed surface & adhesion aid | Clean the plate and apply glue — Bambu Lab lists glue as the way to improve adhesion and prevent warping[20] | Not documented |
| Maximum volumetric flow (mm³/s; see test conditions)mm³/s | 10–16 (PrusaSlicer guidance for ABS/ASA)[21] | Not documented |
| Warping tendency1–5 | High — enclosure needed for reliable large parts; Bambu Lab attributes surface cracking to cooling stress exceeding interlayer adhesion[20] | Not documented |
| Bed-adhesion difficulty1–5 | Needs a specific surface plus adhesive[20] | Not documented |
| Stringing / oozing tendency1–5 | Slight[1] | Not documented |
| Overall printing difficulty1–5 | Intermediate — dry filament and a tuned profile[20][1] | Not documented |
| Extruder requirement | Not documented | Apium states that the adaptive heating system on its industrial machines is what makes POM-C printable, and that no other 3D printer can process it[4] |
| Hardware Wear & Reliability | ||
| Nozzle hardness required1–4 | Brass fine indefinitely[20] | Not documented |
| Abrasiveness1–5 | Non-abrasive[20] | Not documented |
| Nozzle clog risk1–5 | Low — no special hot-end required and clogging is not among the listed drawbacks; Prusa lists no drybox and no hardened nozzle[22][23] | Not documented |
| Heat-creep / jam sensitivity1–5 | Slightly sensitive[22] | Not documented |
| Hotend requirement | No special hot-end required[22] | Not documented |
| Moisture Behaviour | ||
| Moisture absorption (hygroscopicity)1–5 | Moderate — 0.65 % saturated at 25 °C / 55 % RH (Bambu Lab); Polymaker measures 0.51 % maximum uptake for ABS Pro[5][6] | Low (0.1-0.3 %) — extruded POM-C stock takes up 0.18 % in 24 h and 0.80 % at saturation (ASTM D570)[3] |
| Equilibrium moisture content at ~50 % RH% | 0.65 saturated at 25 °C / 55 % RH (Bambu Lab); 0.51 maximum (Polymaker ABS Pro)[5][6] | Not documented |
| Drying temperature & time | 80 °C for 8 h (Bambu Lab); 70 °C for 6 h (Polymaker)[5][1] | Not documented |
| Symptoms when wet | Bubbling and popping at the nozzle, stringing, rough surface and weak layers[24] | Not documented |
| Effect of moisture on strength | Polymaker rates ABS moderate-sensitivity and publishes no dry-versus-conditioned figures; the loss appears as poor layer adhesion and surface defects rather than a stated strength delta[24] | Not documented |
| Storage requirement | Sealed with desiccant; Polymaker rates ABS moderate-sensitivity and advises periodic drying in humid climates[24] | Not documented |
| Mechanical Properties | ||
| Tensile strength (XY)MPa | 33 ± 3 (Bambu Lab) to 35 (Polymaker ABS Pro and Max) printed XY, ISO 527; 3DXTech quotes 42 at break[5][6][7][25] | 66.9 at break and 64.1 at yield (extruded POM-C stock, ASTM D638; converted from 9700 and 9300 psi)[3] |
| Young's modulusMPa | 2200 ± 190 (Bambu Lab) to 2330 (Polymaker ABS Pro) printed XY, ISO 527; 3DXTech quotes 1950[5][6][25] | 2275 (extruded POM-C stock, ASTM D638; converted from 330,000 psi)[3] |
| Elongation at break% | 6.7 (ABS Max) to 10.5 (Bambu Lab) at break, printed XY, ISO 527[5][6][7] | 40 at break and 9 at yield (extruded POM-C stock, ASTM D638)[3] |
| Flexural strengthMPa | 60 (ABS Pro) to 63 (ABS Max) printed XY, ISO 178; Bambu Lab 62 ± 4; 3DXTech quotes 76[5][6][7][25] | 89.6 (extruded POM-C stock, ASTM D790; converted from 13,000 psi)[3] |
| Flexural modulusMPa | 1880 ± 110 (Bambu Lab) to 2500 (ABS Max) printed XY, ISO 178[5][7] | 2758 (extruded POM-C stock, ASTM D790; converted from 400,000 psi)[3] |
| Charpy impact, notchedkJ/m² | 10.5 (ABS Max) and 14.5 (ABS Pro) printed XY, ISO 179, notched; PolyLite ABS 18.0 ± 0.9 and Bambu Lab 21.5 ± 2.2[1][6][7][5] | Not documented |
| Other impact data | Charpy unnotched 39.3 ± 3.6 printed XY (Bambu Lab, ISO 179); notched 21.5 ± 2.2[5] | Izod 53 J/m on extruded POM-C stock, converted from 1.0 ft-lb/in[3] |
| Layer adhesion / Z tensileMPa | 21.9 (ABS Pro) to 29.7 (PolyLite) printed Z, ISO 527; Bambu Lab 28 ± 2[5][1][6] | Not documented |
| Brittleness1–5 | Tough — absorbs impact, yields before breaking[5][1] | Tough — absorbs impact, yields before breaking; extruded stock elongates 40 % before failing. No printed figure is published[3] |
| Hardness (scale-specific)Shore A / Shore D / Rockwell | Not documented | Rockwell 86 (and R120) — the source names only the R scale on extruded POM-C stock (ASTM D785)[3] |
| Creep resistance / sustained load1–5 | Moderate — no printed-ABS creep test found; Tg of 101–126 °C keeps room-temperature service far below softening, unlike PLA[1][6][7] | Not documented |
| Fatigue / repeated-flex resistance1–5 | Moderate — no printed-ABS S-N curve found; 10.5 % elongation and 21.5 kJ/m² notched Charpy give far more cyclic tolerance than PLA[5][26] | Not documented |
| Elasticity / flexibility1–5 | Rigid[5] | Not documented |
| Z strength as % of XY% | 85 (Bambu Lab, printed Z against XY tensile); 63 for Polymaker ABS Pro[5][6] | Not documented |
| Wear resistance & friction | Not documented | Wear factor 65e-10 in3*min/(ft*lb*h) and a dynamic coefficient of friction of 0.21 at 40 psi and 50 fpm (ASTM D3702, extruded stock) — the properties that make acetal the default gear and bushing plastic; Apium lists good sliding properties as the reason for its grade[3][4] |
| Thermal Properties | ||
| HDT at 0.45 MPa°C | 87 (Bambu Lab) to 118 (Polymaker ABS Max), ISO 75 at 0.45 MPa; PolyLite ABS 100[5][1][7] | 158 (extruded POM-C stock, ASTM D648 at 66 psi; converted from 316 °F)[3] |
| HDT at 1.8 MPa°C | 84 (Bambu Lab) to 113 (Polymaker ABS Max), ISO 75 at 1.8 MPa; PolyLite ABS 98[5][1][7] | 110 (extruded POM-C stock, ASTM D648 at 264 psi; converted from 230 °F)[3] |
| Glass transition (Tg)°C | 101 (PolyLite) to 126 (ABS Max), DSC; 105 quoted by 3DXTech[1][7][25] | Not documented |
| Melting point / Vicat°C | Amorphous — no melting point; Vicat 104 (PolyLite) to 127 (ABS Max), ISO 306[1][7] | 165 melting (extruded POM-C stock; converted from 329 °F)[3] |
| Continuous service temperature°C | 101 measured on a loaded glass-filled ABS bar (My Tech Fun); unfilled ABS is bounded by its 84–98 °C heat deflection[27][5][1] | 91 long term and 141 intermittent (extruded POM-C stock; converted from 195 °F and 285 °F)[3] |
| Annealing response | Decomposition above 380 °C (PolyLite ABS, TGA)[1] | Not documented |
| Thermal expansion (CTE)µm/m·K | 86 ± 3 at 0° and 89 ± 3 at 90° raster (printed, fibre Bragg grating, 25–50 °C); 82 for a neat large-format bead at 30 °C[28][29] | 84.6 (extruded POM-C stock, ASTM D696; source states 4.7e-5 in/in/°F)[3] |
| Flammability / UL 94 | Flammable; no UL 94 rating published for standard ABS, though V-0 grades exist[30][5] | UL 94 HB on extruded POM-C stock[3] |
| Environment & Chemical | ||
| UV resistance1–5 | Months outdoors before embrittlement[19] | Not documented |
| Chemical resistance | Good against weak acids, weak alkalis, oils and grease; poor against strong acids; dissolved by acetone[1] | Good chemical resistance, particularly to bases; Apium lists resistance to bases as a headline property[3][4] |
| Water / humidity resistance in service1–5 | Good — minor absorption[5] | Good — minor absorption; 0.80 % water at saturation (ASTM D570, extruded stock)[3] |
| Food contact | Not food safe — Polymaker cites potential chemical leaching[19] | Not documented |
| Biodegradability / compostability | Not biodegradable[19] | Not documented |
| Recyclability | Mechanically recyclable as resin code 9, but not accepted in household plastic collection[19] | Not documented |
| Electrical & ESD properties | Surface resistance above 10¹³ ohm/sq — insulating (3DXTech, ASTM D257)[25] | Volume resistance 1e14 ohm-cm, dielectric strength 500 V/mil and dielectric constant 3.7 at 60 Hz on extruded stock (ASTM D257, D149, D150); Apium's filament grade adds antistatic agents[3][4] |
| Health & Safety | ||
| Fume toxicity1–5 | High — hazardous VOC such as styrene; enclosure and filtration needed[31][20] | Not documented |
| VOC emission rateµg/min | 12–113 styrene, the dominant VOC from every ABS and HIPS combination tested[31] | Not documented |
| Ultrafine-particle emission rateparticles/min | 2 × 10¹⁰ to 9 × 10¹⁰ median across all ABS printers, two orders of magnitude above PLA's ≈1 × 10⁸[31] | Not documented |
| Hazardous species emitted | Styrene dominates. Bambu Lab states ABS and ASA release harmful gases such as styrene at printing temperature, which can be toxic and cause dizziness or nausea[31][20] | Not documented |
| Ventilation / filtration requirement1–5 | Enclosure with carbon and HEPA filtration — an enclosure alone cut measured UFP by only about 35 %[31][20] | Not documented |
| Post-Processing | ||
| Sanding & machining | Sands well and takes filler; the usual preparation before painting[19] | Easy to machine — Ensinger lists machinability as a headline property of POM-C stock[3] |
| Gluing & solvent welding | Solvent-welds with acetone[1] | Not documented |
| Vapour / chemical smoothing | Acetone vapour smoothing works — ABS dissolves in acetone[1] | Not documented |
| Support material pairing | HIPS breaks away or dissolves in d-limonene; Bambu Lab sells a dedicated Support for ABS[32][20] | Not documented |
| Dimensional accuracy & detail | Warping and cooling-stress cracking are the accuracy limits, not shrinkage of the melt[20] | Not documented |
| Solvents & Solubility | ||
| Soluble in | Acetone dissolves it — the basis of ABS slurry; so do MEK, THF, ethyl acetate, chloroform, dichloromethane and toluene.[33][1] | Hexafluoroisopropanol dissolves it at room temperature; NMP and DMF only when hot. Laboratory reagents.[34] |
| Softened or crazed by | Petrol and perchloroethylene soften it and benzene attacks it; d-limonene disrupts layer adhesion in some ABS and ASA grades.[33][35] | Acids, oxidants, halogens and hot concentrated zinc chloride attack it; alcohols, ketones and esters do not.[34][33] |
| Solvent welding & smoothing agent | Acetone: about 20 min of vapour at 80 °C over 5 mm of liquid. Prusa measured layer adhesion more than doubled.[36] | None — no solvent softens POM below its melting point, which is why it is bolted or heat-welded rather than glued.[34] |
Material entries describe families or representative grades, not an interchangeable specification for every spool. Test methods, orientations and conditions may differ. Unknown values are marked “Not documented”. Prices and source dates remain historical snapshots; check the linked guide for product details. Differences highlight text, not a universal winner.
Sources for this comparison
- PolyLite ABS Technical Data Sheet (V5.5 served at this URL) Polymaker · 2024-11 · tds
- Safety Data Sheet SDS20250724B00 — Bambu ABS Bambu Lab · 2025-07 · msds
- TECAFORM AH natural (POM-C) — stock shape properties Ensinger · 2026-08 · tds
- POM-C ESD 3D printing — material page Apium 3D Technologies · 2026-08 · doc
- Bambu Filament Technical Data Sheet V3.0 — ABS Bambu Lab · 2026-08 · tds
- Polymaker ABS Pro Technical Data Sheet V1 (2026-05-29) Polymaker · 2026-05 · tds
- Polymaker ABS Max Technical Data Sheet V1.1 (2026-06-01) Polymaker · 2026-06 · tds
- ABS — product page Bambu Lab US Store · 2026-08 · vendor
- Polymaker product catalogue Polymaker · 2026-08 · vendor
- Push Plastic product catalogue Push Plastic · 2026-08 · vendor
- SUNLU ABS 3D Printer Filament 1 kg SUNLU · 2026-08 · vendor
- IEMAI ABS 3D Printing Filament product page IEMAI 3D · 2026-08 · vendor
- 3DXTech product catalogue 3DXTech · 2026-08 · vendor
- ELEGOO product catalogue ELEGOO · 2026-08 · vendor
- YXPOLYER ABS Squirrel Grey product page YXPOLYER · 2026-08 · vendor
- 3DJAKE product catalogue 3DJAKE · 2026-08 · vendor
- igo3d product sitemap (17452 product URLs) igo3d · 2026-08 · vendor
- Printed Solid product catalogue Printed Solid · 2026-08 · vendor
- ABS — material basics Polymaker Wiki · 2026-08 · doc
- ABS / ASA / PC Usage Guide Bambu Lab Wiki · 2026-08 · doc
- Max volumetric speed Prusa Knowledge Base · 2026-08 · doc
- ABS — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- Filament Material Guide Prusa Knowledge Base · 2026-08 · doc
- Wet Filament — signs, causes and drying Polymaker Wiki · 2026-08 · doc
- 3DXMAX ABS Technical Data Sheet 3DXTech · 2026-08 · tds
- Mechanical Properties of Additively Manufactured Polymeric Materials — PLA and PETG — For Biomechanical Applications Polymers 16(13):1868 · 2024-06 · paper
- ABS-GF vs PET-CF — results spreadsheet My Tech Fun (Igor Gaspar) · 2026-08 · test
- Characterization of Thermal Expansion Coefficient of 3D Printing Polymeric Materials Using Fiber Bragg Grating Sensors Materials 17(18):4668 · 2024-09 · paper
- Effects of Fiber Orientation on the Coefficient of Thermal Expansion of Fiber-Filled Polymer Systems in Large Format Polymer Extrusion-Based Additive Manufacturing Materials 15(8):2764 · 2022-04 · paper
- Firewire Flame Retardant ABS Technical Data Sheet 3DXTech · 2026-08 · tds
- Emissions of Ultrafine Particles and Volatile Organic Compounds from Commercially Available Desktop Three-Dimensional Printers with Multiple Filaments (Azimi et al.) Environmental Science & Technology 50(3) 1260-1268 · 2016-01 · paper
- HIPS — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- Chemical resistance — resistance of Ensinger plastics to chemicals (DIN 50 014, 23/50) Ensinger · 2026-08 · tds
- Resistance of Ultramid, Ultraform and Ultradur to chemicals (TI-KTU/AS-28 e) BASF · 2000-10 · tds
- HIPS — Knowledge Base Prusa Research · 2026-08 · doc