Filament comparison
ABS vs PETG-GF
Compare printing settings, strength, heat resistance, dated prices and sources.
2 selected · all documented properties
| Property | ABSABS | Glass-fibre polyester (PETG-GF / PET-GF)PETG |
|---|---|---|
| Market snapshot | ||
| Listing priceUSD/kg; dated snapshots | $19.99/kg median; $11.99–$45.00/kg across 16 dated product listings | $27.38/kg median; $18.99–$29.99/kg across 3 dated product listings |
| Identity & Market | ||
| Base polymer / chemistry | Acrylonitrile butadiene styrene — a styrenic terpolymer with a butadiene rubber phase[1][2] | Glass-fibre reinforced polyester. Polymaker's Fiberon PET-GF15 uses a PET rather than a PETG matrix and carries 15 wt% glass fibre[3] |
| Densityg/cm³ | 1.04 (Polymaker PolyLite ABS and ABS Pro) to 1.06 (ABS Max), ISO 1183; Bambu Lab 1.05[4][1][5][6] | 1.43 (Fiberon PET-GF15, ISO 1183)[3] |
| Typical priceUSD/kg | 1 kg spools cluster near 20[7][8][9][10][11] | 1 kg spools cluster near 25[12][8] |
| Price range across brandsUSD/kg | 12–45 across brands; IEMAI 12, SUNLU 12 at a 3 kg minimum, ELEGOO 15 in a 5 kg pack, Polymaker 19, YXPOLYER 20, Bambu Lab 20, Push Plastic 25, 3DXTech 45[7][8][13][12][9][10][11][14] | 19–30 across brands; ELEGOO 19, Polymaker Fiberon 30[12][8] |
| Market availability1–5 | Ubiquitous, every brand and retailer[7][8][13][12] | Niche, a handful of specialist brands[12][8] |
| Spool sizes & diameters | 1.75 and 2.85 mm; 1, 5 and 10 kg spools[13][12] | 1.75 mm; 0.5 and 1 kg spools[8] |
| Typical applications | Enclosures, automotive interior parts and tooling that must hold shape above PLA's 55 °C ceiling[1][15] | Stiff, dimensionally stable fixtures; the Fiberon grade is designed to be annealed for heat resistance[3] |
| Printing Parameters | ||
| Nozzle temperature°C | 240–270 (Bambu Lab); 245–265 (Polymaker PolyLite)[4][1] | Not documented |
| Bed temperature°C | 80–100 (Bambu Lab); 90–100 (Polymaker)[4][1] | Not documented |
| Enclosure / chamber requirement1–5 | Enclosure recommended — Polymaker calls a chamber needed at ambient temperature, Bambu Lab requires an enclosed printer and rules out its P1P and A-series machines[1][16] | Not documented |
| Recommended chamber temperature°C | 45–60 (Bambu Lab)[4] | Not documented |
| Part cooling fan | 0–80 % (Bambu Lab); off (Polymaker PolyLite)[4][1] | Not documented |
| Bed surface & adhesion aid | Clean the plate and apply glue — Bambu Lab lists glue as the way to improve adhesion and prevent warping[16] | Textured PEI, satin or powder-coated sheets; on smooth PEI a glue stick acts as a release agent[17][18] |
| Maximum volumetric flow (mm³/s; see test conditions)mm³/s | 10–16 (PrusaSlicer guidance for ABS/ASA)[19] | Not documented |
| Warping tendency1–5 | High — enclosure needed for reliable large parts; Bambu Lab attributes surface cracking to cooling stress exceeding interlayer adhesion[16] | Not documented |
| Bed-adhesion difficulty1–5 | Needs a specific surface plus adhesive[16] | Needs the right surface or a thin adhesive — the problem is releasing the part, not sticking it[17][18] |
| Stringing / oozing tendency1–5 | Slight[1] | Moderate — retraction tuning needed; Polymaker names stringing as PETG's common quirk[18] |
| Overall printing difficulty1–5 | Intermediate — dry filament and a tuned profile[16][1] | Not documented |
| Hardware Wear & Reliability | ||
| Nozzle hardness required1–4 | Brass fine indefinitely[16] | Hardened steel required[3] |
| Abrasiveness1–5 | Non-abrasive[16] | Highly abrasive — standard GF composite[3] |
| Nozzle clog risk1–5 | Low — no special hot-end required and clogging is not among the listed drawbacks; Prusa lists no drybox and no hardened nozzle[20][21] | Moderate — needs dry filament and a clean nozzle; Prusa lists higher risk of nozzle clogging for glass-filled composites[22] |
| Heat-creep / jam sensitivity1–5 | Slightly sensitive[20] | Slightly sensitive[23] |
| Hotend requirement | No special hot-end required[20] | No special hot-end required[23] |
| Moisture Behaviour | ||
| Moisture absorption (hygroscopicity)1–5 | Moderate — 0.65 % saturated at 25 °C / 55 % RH (Bambu Lab); Polymaker measures 0.51 % maximum uptake for ABS Pro[4][5] | Moderate (0.3–0.8 %) — the PETG matrix reaches 0.40 % saturated at 25 °C / 55 % RH; no glass-filled grade publishes its own figure[17] |
| Equilibrium moisture content at ~50 % RH% | 0.65 saturated at 25 °C / 55 % RH (Bambu Lab); 0.51 maximum (Polymaker ABS Pro)[4][5] | Not documented |
| Drying temperature & time | 80 °C for 8 h (Bambu Lab); 70 °C for 6 h (Polymaker)[4][1] | Not documented |
| Symptoms when wet | Bubbling and popping at the nozzle, stringing, rough surface and weak layers[24] | Bubbling and popping at the nozzle, stringing and a rough surface[24] |
| Effect of moisture on strength | Polymaker rates ABS moderate-sensitivity and publishes no dry-versus-conditioned figures; the loss appears as poor layer adhesion and surface defects rather than a stated strength delta[24] | Polymaker groups PETG with nylon, PVA and TPU as highly hygroscopic; no dry-versus-conditioned strength figures are published for this grade and the loss shows as bubbling and poor layer adhesion[24] |
| Storage requirement | Sealed with desiccant; Polymaker rates ABS moderate-sensitivity and advises periodic drying in humid climates[24] | Sealed with desiccant; Polymaker groups PETG with the highly hygroscopic materials[24][18] |
| Mechanical Properties | ||
| Tensile strength (XY)MPa | 33 ± 3 (Bambu Lab) to 35 (Polymaker ABS Pro and Max) printed XY, ISO 527; 3DXTech quotes 42 at break[4][5][6][25] | 59.9 ± 0.8 printed XY, ISO 527 (Fiberon PET-GF15)[3] |
| Young's modulusMPa | 2200 ± 190 (Bambu Lab) to 2330 (Polymaker ABS Pro) printed XY, ISO 527; 3DXTech quotes 1950[4][5][25] | 4144 ± 133 printed XY, ISO 527 (Fiberon PET-GF15)[3] |
| Elongation at break% | 6.7 (ABS Max) to 10.5 (Bambu Lab) at break, printed XY, ISO 527[4][5][6] | 4.0 ± 0.5 printed XY, ISO 527 (Fiberon PET-GF15)[3] |
| Flexural strengthMPa | 60 (ABS Pro) to 63 (ABS Max) printed XY, ISO 178; Bambu Lab 62 ± 4; 3DXTech quotes 76[4][5][6][25] | 104.2 ± 2.4 printed XY, ISO 178 (Fiberon PET-GF15)[3] |
| Flexural modulusMPa | 1880 ± 110 (Bambu Lab) to 2500 (ABS Max) printed XY, ISO 178[4][6] | 3705 ± 85 printed XY, ISO 178 (Fiberon PET-GF15)[3] |
| Charpy impact, notchedkJ/m² | 10.5 (ABS Max) and 14.5 (ABS Pro) printed XY, ISO 179, notched; PolyLite ABS 18.0 ± 0.9 and Bambu Lab 21.5 ± 2.2[1][5][6][4] | 8.7 ± 0.6 printed XY, ISO 179, notched (Fiberon PET-GF15)[3] |
| Other impact data | Charpy unnotched 39.3 ± 3.6 printed XY (Bambu Lab, ISO 179); notched 21.5 ± 2.2[4] | Charpy unnotched 27.2 ± 2.0 printed XY (Fiberon PET-GF15, ISO 179)[3] |
| Layer adhesion / Z tensileMPa | 21.9 (ABS Pro) to 29.7 (PolyLite) printed Z, ISO 527; Bambu Lab 28 ± 2[4][1][5] | 48.2 ± 0.3 printed Z, ISO 527 (Fiberon PET-GF15)[3] |
| Brittleness1–5 | Tough — absorbs impact, yields before breaking[4][1] | Brittle — snaps with little warning; elongation 4.0 % in XY and 2.6 % in Z[3] |
| Creep resistance / sustained load1–5 | Moderate — no printed-ABS creep test found; Tg of 101–126 °C keeps room-temperature service far below softening, unlike PLA[1][5][6] | Below average — no GF-grade creep test; the CF grades sagged to 14.8–16.7 mm over 5 days at 1.25 kg against 17.1–20.4 mm unfilled[26][27][28] |
| Fatigue / repeated-flex resistance1–5 | Moderate — no printed-ABS S-N curve found; 10.5 % elongation and 21.5 kJ/m² notched Charpy give far more cyclic tolerance than PLA[4][29] | Below average — no GF-grade S-N curve; elongation at break falls to 4.0 % in XY against 5.2–9.3 % unfilled[3][29] |
| Elasticity / flexibility1–5 | Rigid[4] | Rigid[3] |
| Z strength as % of XY% | 85 (Bambu Lab, printed Z against XY tensile); 63 for Polymaker ABS Pro[4][5] | 80 (Fiberon PET-GF15, printed Z against XY tensile)[3] |
| Thermal Properties | ||
| HDT at 0.45 MPa°C | 87 (Bambu Lab) to 118 (Polymaker ABS Max), ISO 75 at 0.45 MPa; PolyLite ABS 100[4][1][6] | 81.6 as printed, 133.7 after annealing (ISO 75, 0.45 MPa)[3] |
| HDT at 1.8 MPa°C | 84 (Bambu Lab) to 113 (Polymaker ABS Max), ISO 75 at 1.8 MPa; PolyLite ABS 98[4][1][6] | 71.8 as printed, 87.3 after annealing (ISO 75, 1.8 MPa)[3] |
| Glass transition (Tg)°C | 101 (PolyLite) to 126 (ABS Max), DSC; 105 quoted by 3DXTech[1][6][25] | 59.5 (DSC)[3] |
| Melting point / Vicat°C | Amorphous — no melting point; Vicat 104 (PolyLite) to 127 (ABS Max), ISO 306[1][6] | 231.6 melting (DSC); Vicat 232.6 (ISO 306)[3] |
| Continuous service temperature°C | 101 measured on a loaded glass-filled ABS bar (My Tech Fun); unfilled ABS is bounded by its 84–98 °C heat deflection[30][4][1] | Not documented |
| Annealing response | Decomposition above 380 °C (PolyLite ABS, TGA)[1] | Annealing lifts HDT at 0.45 MPa from 81.6 to 133.7 °C[3] |
| Thermal expansion (CTE)µm/m·K | 86 ± 3 at 0° and 89 ± 3 at 90° raster (printed, fibre Bragg grating, 25–50 °C); 82 for a neat large-format bead at 30 °C[31][32] | 20 along the print bead and 63–74 in the build direction at 30 °C (30 wt% GF, large-format printed, TMA)[32] |
| Flammability / UL 94 | Flammable; no UL 94 rating published for standard ABS, though V-0 grades exist[33][4] | UL 94 HB at 1.5 mm (Fiberon PET-GF15)[3] |
| Environment & Chemical | ||
| UV resistance1–5 | Months outdoors before embrittlement[15] | Not documented |
| Chemical resistance | Good against weak acids, weak alkalis, oils and grease; poor against strong acids; dissolved by acetone[1] | Withstands acids, alkalis, oils and UV exposure[18] |
| Water / humidity resistance in service1–5 | Good — minor absorption[4] | Not documented |
| Food contact | Not food safe — Polymaker cites potential chemical leaching[15] | Not certified for food contact as filament[18] |
| Biodegradability / compostability | Not biodegradable[15] | Not biodegradable[18] |
| Recyclability | Mechanically recyclable as resin code 9, but not accepted in household plastic collection[15] | Not accepted in household plastic collection[18] |
| Electrical & ESD properties | Surface resistance above 10¹³ ohm/sq — insulating (3DXTech, ASTM D257)[25] | Surface resistivity above 10¹² ohm — insulating (Fiberon PET-GF15, ANSI/ESD S11.11)[3] |
| Health & Safety | ||
| Fume toxicity1–5 | High — hazardous VOC such as styrene; enclosure and filtration needed[34][16] | Moderate — measurable VOCs and UFPs, ventilation advised[34] |
| VOC emission rateµg/min | 12–113 styrene, the dominant VOC from every ABS and HIPS combination tested[34] | Not documented |
| Ultrafine-particle emission rateparticles/min | 2 × 10¹⁰ to 9 × 10¹⁰ median across all ABS printers, two orders of magnitude above PLA's ≈1 × 10⁸[34] | Not documented |
| Hazardous species emitted | Styrene dominates. Bambu Lab states ABS and ASA release harmful gases such as styrene at printing temperature, which can be toxic and cause dizziness or nausea[34][16] | Not documented |
| Ventilation / filtration requirement1–5 | Enclosure with carbon and HEPA filtration — an enclosure alone cut measured UFP by only about 35 %[34][16] | Open a window / occasional ventilation[34] |
| Dust & fibre handling hazard | Not documented | Glass fibre is bound in the matrix; avoid inhaling sanding dust[3] |
| Post-Processing | ||
| Sanding & machining | Sands well and takes filler; the usual preparation before painting[15] | Sands poorly — the material is tough and gums rather than powders[23] |
| Gluing & solvent welding | Solvent-welds with acetone[1] | Cyanoacrylate; no common solvent welds PETG cleanly[23] |
| Vapour / chemical smoothing | Acetone vapour smoothing works — ABS dissolves in acetone[1] | No practical vapour smoothing[23] |
| Support material pairing | HIPS breaks away or dissolves in d-limonene; Bambu Lab sells a dedicated Support for ABS[35][16] | Prints its own supports; Polymaker rates PolyDissolve S1 for PETG[23] |
| Dimensional accuracy & detail | Warping and cooling-stress cracking are the accuracy limits, not shrinkage of the melt[16] | Not documented |
| Solvents & Solubility | ||
| Soluble in | Acetone dissolves it — the basis of ABS slurry; so do MEK, THF, ethyl acetate, chloroform, dichloromethane and toluene.[36][1] | No common workshop solvent; dichloromethane — a carcinogen — dissolves the matrix surface, 1,2-dichloroethane destroys it in a week.[37][38] |
| Softened or crazed by | Petrol and perchloroethylene soften it and benzene attacks it; d-limonene disrupts layer adhesion in some ABS and ASA grades.[36][39] | Acetone (+16 % weight over 1 year at 23 °C), ethyl acetate, toluene and DMF swell and soften it; methanol crazes it.[37] |
| Solvent welding & smoothing agent | Acetone: about 20 min of vapour at 80 °C over 5 mm of liquid. Prusa measured layer adhesion more than doubled.[38] | Dichloromethane reaches only the resin, so the fibre is left standing proud of the surface. Controlled carcinogen.[38] |
Material entries describe families or representative grades, not an interchangeable specification for every spool. Test methods, orientations and conditions may differ. Unknown values are marked “Not documented”. Prices and source dates remain historical snapshots; check the linked guide for product details. Differences highlight text, not a universal winner.
Sources for this comparison
- PolyLite ABS Technical Data Sheet (V5.5 served at this URL) Polymaker · 2024-11 · tds
- Safety Data Sheet SDS20250724B00 — Bambu ABS Bambu Lab · 2025-07 · msds
- Fiberon PET-GF15 Technical Data Sheet V1.0 Polymaker · 2026-08 · tds
- Bambu Filament Technical Data Sheet V3.0 — ABS Bambu Lab · 2026-08 · tds
- Polymaker ABS Pro Technical Data Sheet V1 (2026-05-29) Polymaker · 2026-05 · tds
- Polymaker ABS Max Technical Data Sheet V1.1 (2026-06-01) Polymaker · 2026-06 · tds
- ABS — product page Bambu Lab US Store · 2026-08 · vendor
- Polymaker product catalogue Polymaker · 2026-08 · vendor
- Push Plastic product catalogue Push Plastic · 2026-08 · vendor
- SUNLU ABS 3D Printer Filament 1 kg SUNLU · 2026-08 · vendor
- IEMAI ABS 3D Printing Filament product page IEMAI 3D · 2026-08 · vendor
- ELEGOO product catalogue ELEGOO · 2026-08 · vendor
- 3DXTech product catalogue 3DXTech · 2026-08 · vendor
- YXPOLYER ABS Squirrel Grey product page YXPOLYER · 2026-08 · vendor
- ABS — material basics Polymaker Wiki · 2026-08 · doc
- ABS / ASA / PC Usage Guide Bambu Lab Wiki · 2026-08 · doc
- Prusament PETG Technical Datasheet v1.1 Prusa Polymers · 2022-02 · tds
- PETG — material basics Polymaker Wiki · 2026-08 · doc
- Max volumetric speed Prusa Knowledge Base · 2026-08 · doc
- ABS — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- Filament Material Guide Prusa Knowledge Base · 2026-08 · doc
- Composite materials filled with carbon, kevlar or glass Prusa Knowledge Base · 2026-08 · doc
- PET and PETG — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- Wet Filament — signs, causes and drying Polymaker Wiki · 2026-08 · doc
- 3DXMAX ABS Technical Data Sheet 3DXTech · 2026-08 · tds
- Extrudr PETG vs PCTG vs XPETG-CF — results spreadsheet My Tech Fun (Igor Gaspar) · 2026-08 · test
- Prusament PETG-CF vs PETG V0 vs PETG — results spreadsheet My Tech Fun (Igor Gaspar) · 2026-08 · test
- BambuLab PETG Basic vs Translucent vs PETG-CF — results spreadsheet My Tech Fun (Igor Gaspar) · 2026-08 · test
- Mechanical Properties of Additively Manufactured Polymeric Materials — PLA and PETG — For Biomechanical Applications Polymers 16(13):1868 · 2024-06 · paper
- ABS-GF vs PET-CF — results spreadsheet My Tech Fun (Igor Gaspar) · 2026-08 · test
- Characterization of Thermal Expansion Coefficient of 3D Printing Polymeric Materials Using Fiber Bragg Grating Sensors Materials 17(18):4668 · 2024-09 · paper
- Effects of Fiber Orientation on the Coefficient of Thermal Expansion of Fiber-Filled Polymer Systems in Large Format Polymer Extrusion-Based Additive Manufacturing Materials 15(8):2764 · 2022-04 · paper
- Firewire Flame Retardant ABS Technical Data Sheet 3DXTech · 2026-08 · tds
- Emissions of Ultrafine Particles and Volatile Organic Compounds from Commercially Available Desktop Three-Dimensional Printers with Multiple Filaments (Azimi et al.) Environmental Science & Technology 50(3) 1260-1268 · 2016-01 · paper
- HIPS — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- Chemical resistance — resistance of Ensinger plastics to chemicals (DIN 50 014, 23/50) Ensinger · 2026-08 · tds
- Eastman Spectar copolyester — Chemical resistance (unstressed bars, 1 year at 23 °C) Eastman Chemical Company · 2026-08 · tds
- Improve your 3D prints with chemical smoothing Prusa Research · 2026-08 · doc
- HIPS — Knowledge Base Prusa Research · 2026-08 · doc