| Property | ABSABS | Carbon-fibre ASA (ASA-CF)ASA |
|---|---|---|
| Market snapshot | ||
| Listing priceUSD/kg; dated snapshots | $19.99/kg median; $11.99–$45.00/kg across 16 dated product listings | $36.99/kg median; $25.00–$90.00/kg across 5 dated product listings |
| Identity & Market | ||
| Base polymer / chemistry | Acrylonitrile butadiene styrene — a styrenic terpolymer with a butadiene rubber phase[1][2] | ASA reinforced with chopped carbon fibre — Formfutura's ApolloX CF10 is 10 wt%[3][4][5] |
| Densityg/cm³ | 1.04 (Polymaker PolyLite ABS and ABS Pro) to 1.06 (ABS Max), ISO 1183; Bambu Lab 1.05[6][1][7][8] | 1.02 (Bambu Lab), 1.1 (Formfutura ApolloX CF10) and 1.11 (3DXTech), ISO 1183[3][4][5] |
| Typical priceUSD/kg | 1 kg spools cluster near 20[9][10][11][12][13] | 1 kg spools cluster near 37[14][10] |
| Price range across brandsUSD/kg | 12–45 across brands; IEMAI 12, SUNLU 12 at a 3 kg minimum, ELEGOO 15 in a 5 kg pack, Polymaker 19, YXPOLYER 20, Bambu Lab 20, Push Plastic 25, 3DXTech 45[9][10][15][16][11][12][13][17] | 25–90 across brands; IEMAI 25, Ambrosia 33, Bambu Lab 37, Polymaker Fiberon 40, 3DXTech 90[18][14][10][15][19] |
| Market availability1–5 | Ubiquitous, every brand and retailer[9][10][15][16] | Available from several mainstream brands[14][10][15][18] |
| Spool sizes & diameters | 1.75 and 2.85 mm; 1, 5 and 10 kg spools[15][16] | 1.75 and 2.85 mm; 0.5, 0.75 and 1 kg spools[10][15][14] |
| Typical applications | Enclosures, automotive interior parts and tooling that must hold shape above PLA's 55 °C ceiling[1][20] | Outdoor structural parts, drone and antenna mounts where stiffness and UV stability both matter[3][4] |
| Printing Parameters | ||
| Nozzle temperature°C | 240–270 (Bambu Lab); 245–265 (Polymaker PolyLite)[6][1] | 250–280 (Bambu Lab)[3] |
| Bed temperature°C | 80–100 (Bambu Lab); 90–100 (Polymaker)[6][1] | 80–100 (Bambu Lab)[3] |
| Enclosure / chamber requirement1–5 | Enclosure recommended — Polymaker calls a chamber needed at ambient temperature, Bambu Lab requires an enclosed printer and rules out its P1P and A-series machines[1][21] | Enclosure recommended — Bambu Lab specifies a 45–60 °C chamber[3][21] |
| Recommended chamber temperature°C | 45–60 (Bambu Lab)[6] | 45–60 (Bambu Lab)[3] |
| Part cooling fan | 0–80 % (Bambu Lab); off (Polymaker PolyLite)[6][1] | Fan on (Bambu Lab)[3] |
| Bed surface & adhesion aid | Clean the plate and apply glue — Bambu Lab lists glue as the way to improve adhesion and prevent warping[21] | PEI sheet, BuildTak or an adhesion aid such as Magigoo (Polymaker); Simplify3D also lists Kapton tape and ASA slurry[22][23] |
| Maximum volumetric flow (mm³/s; see test conditions)mm³/s | 10–16 (PrusaSlicer guidance for ABS/ASA)[24] | 20 at Bambu Lab's 250 mm/s cap on a 0.4 mm nozzle at 0.2 mm layer[3][24] |
| Warping tendency1–5 | High — enclosure needed for reliable large parts; Bambu Lab attributes surface cracking to cooling stress exceeding interlayer adhesion[21] | Moderate — needs adhesion aid or draught shield; the fibre reduces warping against unfilled ASA[21] |
| Bed-adhesion difficulty1–5 | Needs a specific surface plus adhesive[21] | Needs a specific surface plus adhesive[22] |
| Stringing / oozing tendency1–5 | Slight[1] | Slight — Polymaker advises 1–2 mm retraction at 20–30 mm/s[22] |
| Overall printing difficulty1–5 | Intermediate — dry filament and a tuned profile[21][1] | Intermediate — dry filament and a tuned profile; hardened nozzle mandatory[21] |
| Hardware Wear & Reliability | ||
| Nozzle hardness required1–4 | Brass fine indefinitely[21] | Hardened steel required[21] |
| Abrasiveness1–5 | Non-abrasive[21] | Highly abrasive — standard CF composite[21] |
| Nozzle clog risk1–5 | Low — no special hot-end required and clogging is not among the listed drawbacks; Prusa lists no drybox and no hardened nozzle[25][26] | Moderate — needs dry filament and a clean nozzle; Prusa lists higher risk of nozzle clogging for fibre-filled composites and Simplify3D a higher tendency to clog[27][28] |
| Heat-creep / jam sensitivity1–5 | Slightly sensitive[25] | Slightly sensitive[23] |
| Hotend requirement | No special hot-end required[25] | No special hotend required[23] |
| Moisture Behaviour | ||
| Moisture absorption (hygroscopicity)1–5 | Moderate — 0.65 % saturated at 25 °C / 55 % RH (Bambu Lab); Polymaker measures 0.51 % maximum uptake for ABS Pro[6][7] | Moderate — 0.33 % saturated at 25 °C / 55 % RH (Bambu Lab)[3] |
| Equilibrium moisture content at ~50 % RH% | 0.65 saturated at 25 °C / 55 % RH (Bambu Lab); 0.51 maximum (Polymaker ABS Pro)[6][7] | 0.33 saturated at 25 °C / 55 % RH (Bambu Lab)[3] |
| Drying temperature & time | 80 °C for 8 h (Bambu Lab); 70 °C for 6 h (Polymaker)[6][1] | 80 °C for 8 h (Bambu Lab)[3] |
| Symptoms when wet | Bubbling and popping at the nozzle, stringing, rough surface and weak layers[29] | Bubbling and popping at the nozzle, stringing and a rough surface[29] |
| Effect of moisture on strength | Polymaker rates ABS moderate-sensitivity and publishes no dry-versus-conditioned figures; the loss appears as poor layer adhesion and surface defects rather than a stated strength delta[29] | No dry-versus-conditioned figures are published; Polymaker groups the styrenics as moderate-sensitivity and absorbed water shows as bubbling and poor layer adhesion[29] |
| Storage requirement | Sealed with desiccant; Polymaker rates ABS moderate-sensitivity and advises periodic drying in humid climates[29] | Sealed with desiccant; Polymaker rates the styrenics moderate-sensitivity[29] |
| Mechanical Properties | ||
| Tensile strength (XY)MPa | 33 ± 3 (Bambu Lab) to 35 (Polymaker ABS Pro and Max) printed XY, ISO 527; 3DXTech quotes 42 at break[6][7][8][30] | 34 ± 3 printed XY, ISO 527 (Bambu Lab); 3DXTech quotes 48 at break and Formfutura 79 at 23 °C[3][4][5] |
| Young's modulusMPa | 2200 ± 190 (Bambu Lab) to 2330 (Polymaker ABS Pro) printed XY, ISO 527; 3DXTech quotes 1950[6][7][30] | 4200 ± 270 printed XY, ISO 527 (Bambu Lab); 3DXTech quotes 5355 and Formfutura 7580[3][4][5] |
| Elongation at break% | 6.7 (ABS Max) to 10.5 (Bambu Lab) at break, printed XY, ISO 527[6][7][8] | 9.6 ± 1.4 printed XY, ISO 527 (Bambu Lab); 3DXTech quotes 3 at break and Formfutura 1.8[3][4][5] |
| Flexural strengthMPa | 60 (ABS Pro) to 63 (ABS Max) printed XY, ISO 178; Bambu Lab 62 ± 4; 3DXTech quotes 76[6][7][8][30] | 72 ± 5 printed XY, ISO 178 (Bambu Lab); 3DXTech quotes 78[3][4] |
| Flexural modulusMPa | 1880 ± 110 (Bambu Lab) to 2500 (ABS Max) printed XY, ISO 178[6][8] | 3740 ± 130 printed XY, ISO 178 (Bambu Lab); 3DXTech quotes 5210[3][4] |
| Charpy impact, notchedkJ/m² | 10.5 (ABS Max) and 14.5 (ABS Pro) printed XY, ISO 179, notched; PolyLite ABS 18.0 ± 0.9 and Bambu Lab 21.5 ± 2.2[1][7][8][6] | 6.2 ± 1.4 printed XY, ISO 179, notched (Bambu Lab) — a third of unfilled Bambu Lab ASA's 19.6[3][31] |
| Other impact data | Charpy unnotched 39.3 ± 3.6 printed XY (Bambu Lab, ISO 179); notched 21.5 ± 2.2[6] | Charpy unnotched 14.0 ± 2.2 printed XY (Bambu Lab, ISO 179), against 41.0 for unfilled Bambu Lab ASA[3][31] |
| Layer adhesion / Z tensileMPa | 21.9 (ABS Pro) to 29.7 (PolyLite) printed Z, ISO 527; Bambu Lab 28 ± 2[6][1][7] | 30 ± 4 printed Z, ISO 527 (Bambu Lab); flexural Z falls to 33 against 72 in XY[3] |
| Brittleness1–5 | Tough — absorbs impact, yields before breaking[6][1] | Brittle — snaps with little warning[3][4] |
| Creep resistance / sustained load1–5 | Moderate — no printed-ABS creep test found; Tg of 101–126 °C keeps room-temperature service far below softening, unlike PLA[1][7][8] | Good — no creep test found; chopped carbon fibre lifts modulus to 4200 MPa against 2379–2450 for unfilled ASA[3][32] |
| Fatigue / repeated-flex resistance1–5 | Moderate — no printed-ABS S-N curve found; 10.5 % elongation and 21.5 kJ/m² notched Charpy give far more cyclic tolerance than PLA[6][33] | Below average — no CF-grade S-N curve; notched Charpy falls to 6.2 kJ/m² against 19.6 for unfilled Bambu Lab ASA[3][31] |
| Elasticity / flexibility1–5 | Rigid[6] | Rigid[3] |
| Z strength as % of XY% | 85 (Bambu Lab, printed Z against XY tensile); 63 for Polymaker ABS Pro[6][7] | 88 by tensile, 46 by flexural (printed, Bambu Lab)[3] |
| Thermal Properties | ||
| HDT at 0.45 MPa°C | 87 (Bambu Lab) to 118 (Polymaker ABS Max), ISO 75 at 0.45 MPa; PolyLite ABS 100[6][1][8] | 110 (ISO 75, 0.45 MPa, Bambu Lab) against 100 for unfilled Bambu Lab ASA[3][31] |
| HDT at 1.8 MPa°C | 84 (Bambu Lab) to 113 (Polymaker ABS Max), ISO 75 at 1.8 MPa; PolyLite ABS 98[6][1][8] | 102 (ISO 75, 1.8 MPa, Bambu Lab) against 92 for unfilled Bambu Lab ASA[3][31] |
| Glass transition (Tg)°C | 101 (PolyLite) to 126 (ABS Max), DSC; 105 quoted by 3DXTech[1][8][30] | Not documented |
| Melting point / Vicat°C | Amorphous — no melting point; Vicat 104 (PolyLite) to 127 (ABS Max), ISO 306[1][8] | Not documented |
| Continuous service temperature°C | 101 measured on a loaded glass-filled ABS bar (My Tech Fun); unfilled ABS is bounded by its 84–98 °C heat deflection[34][6][1] | 93 — Prusa publishes this as the temperature resistance of Prusament ASA[35] |
| Annealing response | Decomposition above 380 °C (PolyLite ABS, TGA)[1] | Not documented |
| Thermal expansion (CTE)µm/m·K | 86 ± 3 at 0° and 89 ± 3 at 90° raster (printed, fibre Bragg grating, 25–50 °C); 82 for a neat large-format bead at 30 °C[36][37] | Not documented |
| Flammability / UL 94 | Flammable; no UL 94 rating published for standard ABS, though V-0 grades exist[38][6] | Flammable; no UL 94 rating published[31] |
| Environment & Chemical | ||
| UV resistance1–5 | Months outdoors before embrittlement[20] | Excellent — designed for permanent outdoor use; the acrylate rubber phase is unchanged by the fibre[39][22] |
| Chemical resistance | Good against weak acids, weak alkalis, oils and grease; poor against strong acids; dissolved by acetone[1] | Good against weak acids, weak alkalis, oils and grease; dissolved by acetone[32] |
| Water / humidity resistance in service1–5 | Good — minor absorption[6] | Not documented |
| Food contact | Not food safe — Polymaker cites potential chemical leaching[20] | Not food safe[22] |
| Biodegradability / compostability | Not biodegradable[20] | Not biodegradable[22] |
| Recyclability | Mechanically recyclable as resin code 9, but not accepted in household plastic collection[20] | Not accepted in household plastic collection[22] |
| Electrical & ESD properties | Surface resistance above 10¹³ ohm/sq — insulating (3DXTech, ASTM D257)[30] | Surface resistance above 10⁹ ohm/sq — not static-dissipative (3DXTech, ASTM D257)[4] |
| Health & Safety | ||
| Fume toxicity1–5 | High — hazardous VOC such as styrene; enclosure and filtration needed[40][21] | High — hazardous VOC such as styrene; enclosure and filtration needed[40][21] |
| VOC emission rateµg/min | 12–113 styrene, the dominant VOC from every ABS and HIPS combination tested[40] | Not documented |
| Ultrafine-particle emission rateparticles/min | 2 × 10¹⁰ to 9 × 10¹⁰ median across all ABS printers, two orders of magnitude above PLA's ≈1 × 10⁸[40] | Not documented |
| Hazardous species emitted | Styrene dominates. Bambu Lab states ABS and ASA release harmful gases such as styrene at printing temperature, which can be toxic and cause dizziness or nausea[40][21] | Styrene. Bambu Lab states ABS and ASA release harmful gases such as styrene at printing temperature, which can be toxic and cause dizziness or nausea. Azimi et al. measured styrene from every styrenic filament tested but did not test ASA itself[21][40] |
| Ventilation / filtration requirement1–5 | Enclosure with carbon and HEPA filtration — an enclosure alone cut measured UFP by only about 35 %[40][21] | Enclosure with carbon and HEPA filtration[40][21] |
| Dust & fibre handling hazard | Not documented | Carbon fibre is bound in the matrix; sanding dust should not be inhaled[4] |
| Post-Processing | ||
| Sanding & machining | Sands well and takes filler; the usual preparation before painting[20] | Sands well and takes filler before painting[22] |
| Painting & finishing | Not documented | Paints readily; ASA holds colour outdoors so many parts are left unpainted[22] |
| Gluing & solvent welding | Solvent-welds with acetone[1] | Solvent-welds with acetone[32] |
| Vapour / chemical smoothing | Acetone vapour smoothing works — ABS dissolves in acetone[1] | Acetone vapour smoothing works[32] |
| Support material pairing | HIPS breaks away or dissolves in d-limonene; Bambu Lab sells a dedicated Support for ABS[41][21] | HIPS breaks away or dissolves in d-limonene; Bambu Lab sells a Support for ABS that also serves ASA[21] |
| Dimensional accuracy & detail | Warping and cooling-stress cracking are the accuracy limits, not shrinkage of the melt[21] | Matte fibre-filled finish hides layer lines[3] |
| Solvents & Solubility | ||
| Soluble in | Acetone dissolves it — the basis of ABS slurry; so do MEK, THF, ethyl acetate, chloroform, dichloromethane and toluene.[42][1] | Acetone dissolves the resin and leaves the fibre; MEK, THF, ethyl acetate and chlorinated solvents attack the styrenic backbone.[42][32] |
| Softened or crazed by | Petrol and perchloroethylene soften it and benzene attacks it; d-limonene disrupts layer adhesion in some ABS and ASA grades.[42][43] | Limonene attacks some grades — Prusa reports Prusament ASA Orange flaking apart as layer adhesion fails.[43] |
| Solvent welding & smoothing agent | Acetone: about 20 min of vapour at 80 °C over 5 mm of liquid. Prusa measured layer adhesion more than doubled.[44] | Acetone vapour reaches only the resin fraction, so the fibre is left standing proud of the smoothed surface.[44][32] |
Material entries describe families or representative grades, not an interchangeable specification for every spool. Test methods, orientations and conditions may differ. Unknown values are marked “Not documented”. Prices and source dates remain historical snapshots; check the linked guide for product details. Differences highlight text, not a universal winner.
Sources for this comparison
- PolyLite ABS Technical Data Sheet (V5.5 served at this URL) Polymaker · 2024-11 · tds
- Safety Data Sheet SDS20250724B00 — Bambu ABS Bambu Lab · 2025-07 · msds
- Bambu Filament Technical Data Sheet V1.0 — ASA-CF Bambu Lab · 2026-08 · tds
- CarbonX Carbon Fiber ASA Technical Data Sheet 3DXTech · 2026-08 · tds
- ApolloX CF10 Technical Data Sheet Formfutura · 2026-08 · tds
- Bambu Filament Technical Data Sheet V3.0 — ABS Bambu Lab · 2026-08 · tds
- Polymaker ABS Pro Technical Data Sheet V1 (2026-05-29) Polymaker · 2026-05 · tds
- Polymaker ABS Max Technical Data Sheet V1.1 (2026-06-01) Polymaker · 2026-06 · tds
- ABS — product page Bambu Lab US Store · 2026-08 · vendor
- Polymaker product catalogue Polymaker · 2026-08 · vendor
- Push Plastic product catalogue Push Plastic · 2026-08 · vendor
- SUNLU ABS 3D Printer Filament 1 kg SUNLU · 2026-08 · vendor
- IEMAI ABS 3D Printing Filament product page IEMAI 3D · 2026-08 · vendor
- ASA-CF — product page Bambu Lab US Store · 2026-08 · vendor
- 3DXTech product catalogue 3DXTech · 2026-08 · vendor
- ELEGOO product catalogue ELEGOO · 2026-08 · vendor
- YXPOLYER ABS Squirrel Grey product page YXPOLYER · 2026-08 · vendor
- Filastruder product catalogue Filastruder · 2026-08 · vendor
- IEMAI CF-ASA 3D Printing Filament product page IEMAI 3D · 2026-08 · vendor
- ABS — material basics Polymaker Wiki · 2026-08 · doc
- ABS / ASA / PC Usage Guide Bambu Lab Wiki · 2026-08 · doc
- ASA — material basics Polymaker Wiki · 2026-08 · doc
- ASA — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- Max volumetric speed Prusa Knowledge Base · 2026-08 · doc
- ABS — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- Filament Material Guide Prusa Knowledge Base · 2026-08 · doc
- Composite materials filled with carbon, kevlar or glass Prusa Knowledge Base · 2026-08 · doc
- Carbon Fiber Filled — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- Wet Filament — signs, causes and drying Polymaker Wiki · 2026-08 · doc
- 3DXMAX ABS Technical Data Sheet 3DXTech · 2026-08 · tds
- Bambu Filament Technical Data Sheet V3.0 — ASA Bambu Lab · 2026-08 · tds
- PolyLite ASA Technical Data Sheet Polymaker · 2024-11 · tds
- Mechanical Properties of Additively Manufactured Polymeric Materials — PLA and PETG — For Biomechanical Applications Polymers 16(13):1868 · 2024-06 · paper
- ABS-GF vs PET-CF — results spreadsheet My Tech Fun (Igor Gaspar) · 2026-08 · test
- Prusament ASA — material page Prusa Polymers · 2026-08 · doc
- Characterization of Thermal Expansion Coefficient of 3D Printing Polymeric Materials Using Fiber Bragg Grating Sensors Materials 17(18):4668 · 2024-09 · paper
- Effects of Fiber Orientation on the Coefficient of Thermal Expansion of Fiber-Filled Polymer Systems in Large Format Polymer Extrusion-Based Additive Manufacturing Materials 15(8):2764 · 2022-04 · paper
- Firewire Flame Retardant ABS Technical Data Sheet 3DXTech · 2026-08 · tds
- ASA — FDM Material Data Sheet (includes 1000 h QUV exposure results) Stratasys · 2026-08 · tds
- Emissions of Ultrafine Particles and Volatile Organic Compounds from Commercially Available Desktop Three-Dimensional Printers with Multiple Filaments (Azimi et al.) Environmental Science & Technology 50(3) 1260-1268 · 2016-01 · paper
- HIPS — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- Chemical resistance — resistance of Ensinger plastics to chemicals (DIN 50 014, 23/50) Ensinger · 2026-08 · tds
- HIPS — Knowledge Base Prusa Research · 2026-08 · doc
- Improve your 3D prints with chemical smoothing Prusa Research · 2026-08 · doc