Filament comparison
ABS-GF vs ABS+
Compare printing settings, strength, heat resistance, dated prices and sources.
2 selected · all documented properties
| Property | Glass-fibre ABS (ABS-GF)ABS | ABS+ / Tough ABSABS |
|---|---|---|
| Market snapshot | ||
| Listing priceUSD/kg; dated snapshots | $34.99/kg median; $24.49–$73.33/kg across 4 dated product listings | $26.49/kg median; $15.99–$29.99/kg across 4 dated product listings |
| Identity & Market | ||
| Base polymer / chemistry | ABS reinforced with chopped glass fibre — 3DXTech's grade is nominally 10 wt%[1][2] | ABS reformulated for lower warping and a higher glass transition; Polymaker's ABS Pro and ABS Max reach Tg 114.9 and 126.3 °C against 101 °C for PolyLite ABS[3][4][5] |
| Densityg/cm³ | 1.08 (Bambu Lab) and 1.15 (3DXTech), ISO 1183[2][1] | 1.04 (ABS Pro) and 1.06 (ABS Max), ISO 1183[3][4] |
| Typical priceUSD/kg | 1 kg-equivalent spools span 24–73; the middle of the market is about 35[6][7][8][9] | 1 kg spools cluster near 27[10] |
| Price range across brandsUSD/kg | 24–73 across brands; Siraya Tech 24, Bambu Lab 30, SUNLU 40, 3DXTech 73[6][7][8][9] | 16–30 across brands; SUNLU E-ABS 16, Polymaker ABS Pro 25, YXPOLYER ABS Enhanced 28, Polymaker ABS Max 30[10][11][12] |
| Market availability1–5 | Available from several mainstream brands[6][7] | Available from several mainstream brands[10] |
| Spool sizes & diameters | 1.75 and 2.85 mm; 750 g and 1 kg spools[7][6] | 1.75 and 2.85 mm; 1 kg spools[10] |
| Typical applications | Stiff, dimensionally stable enclosure and tooling parts; Bambu Lab notes the fibre blurs layer lines into a matte finish[2] | Large enclosure and automotive parts where plain ABS warps or softens too early[3][4] |
| Printing Parameters | ||
| Nozzle temperature°C | 240–280 (Bambu Lab)[2] | 270–290 (ABS Pro); 270–300 (ABS Max) — 25–35 °C above plain ABS[3][4] |
| Bed temperature°C | 80–100 (Bambu Lab)[2] | 120 (ABS Max)[4] |
| Enclosure / chamber requirement1–5 | Enclosure recommended — Bambu Lab specifies a 45–60 °C chamber[2][13] | Enclosure required (passive)[3][4][13] |
| Recommended chamber temperature°C | 45–60 (Bambu Lab)[2] | Not documented |
| Part cooling fan | 0–80 % (Bambu Lab)[2] | Not documented |
| Bed surface & adhesion aid | Clean the plate and apply glue; Simplify3D also lists Kapton tape and ABS slurry[13][14] | Clean the plate and apply glue; Simplify3D also lists Kapton tape and ABS slurry[13][14] |
| Maximum volumetric flow (mm³/s; see test conditions)mm³/s | 14 at Bambu Lab's 180 mm/s cap on a 0.4 mm nozzle at 0.2 mm layer[2][15] | Up to 250 mm/s (ABS Pro) and 200 mm/s (ABS Max), equivalent to 20 and 16 on a 0.4 mm nozzle at 0.2 mm layer[3][4][15] |
| Warping tendency1–5 | Moderate — needs adhesion aid or draught shield; Bambu Lab positions the fibre as reducing warping[2] | High — enclosure needed for reliable large parts[13] |
| Bed-adhesion difficulty1–5 | Needs a specific surface plus adhesive[13] | Needs a specific surface plus adhesive[13] |
| Stringing / oozing tendency1–5 | Slight — Polymaker advises 1–2 mm retraction at 20–30 mm/s[16] | Slight — Polymaker advises 1–2 mm retraction at 20–30 mm/s[16] |
| Overall printing difficulty1–5 | Intermediate — dry filament and a tuned profile; hardened nozzle mandatory[13] | Intermediate — dry filament and a tuned profile; the hotter nozzle rules out PTFE-lined hotends[3][4] |
| Hardware Wear & Reliability | ||
| Nozzle hardness required1–4 | Hardened steel required[13] | Brass fine indefinitely[13] |
| Abrasiveness1–5 | Highly abrasive — standard GF composite[13] | Non-abrasive[13] |
| Nozzle clog risk1–5 | Moderate — needs dry filament and a clean nozzle; 3DXTech specifies a hardened 0.4 mm minimum nozzle and 0.25 mm layers or higher for the glass-filled grade[17][18] | Low — unfilled ABS compound; no special hot-end required and clogging is not among the listed drawbacks[14][19] |
| Heat-creep / jam sensitivity1–5 | Slightly sensitive[14] | Slightly sensitive[14] |
| Hotend requirement | No special hot-end required[14] | No special hot-end required[14] |
| Moisture Behaviour | ||
| Moisture absorption (hygroscopicity)1–5 | Moderate — 0.53 % saturated at 25 °C / 55 % RH (Bambu Lab)[2] | Moderate — 0.51 % maximum water absorption (ABS Pro)[3] |
| Equilibrium moisture content at ~50 % RH% | 0.53 saturated at 25 °C / 55 % RH (Bambu Lab)[2] | 0.51 maximum water absorption (Polymaker ABS Pro)[3] |
| Drying temperature & time | 80 °C for 8 h (Bambu Lab)[2] | 70 °C for 6 h (ABS Max)[4] |
| Symptoms when wet | Bubbling and popping at the nozzle, stringing and a rough surface[20] | Bubbling and popping at the nozzle, stringing and a rough surface[20] |
| Effect of moisture on strength | Polymaker rates ABS moderate-sensitivity and publishes no dry-versus-conditioned figures; absorbed water flashes to steam in the hotend and shows as bubbling and poor layer adhesion[20] | Polymaker rates ABS moderate-sensitivity and publishes no dry-versus-conditioned figures[20] |
| Storage requirement | Sealed with desiccant; Polymaker rates ABS moderate-sensitivity[20] | Sealed with desiccant; Polymaker rates ABS moderate-sensitivity[20] |
| Mechanical Properties | ||
| Tensile strength (XY)MPa | 36 ± 3 printed XY, ISO 527 (Bambu Lab); 3DXTech quotes 68 at break[2][1] | 34.9 (ABS Pro) and 35.7 (ABS Max) printed XY, ISO 527[3][4] |
| Young's modulusMPa | 3160 ± 170 printed XY, ISO 527 (Bambu Lab); 3DXTech quotes 4210[2][1] | 2330 (ABS Pro) and 2320 (ABS Max) printed XY, ISO 527[3][4] |
| Elongation at break% | 6.3 ± 1.2 printed XY, ISO 527 (Bambu Lab); 3DXTech quotes 2 at break[2][1] | 6.7 (ABS Max) and 7.3 (ABS Pro) at break, printed XY, ISO 527[3][4] |
| Flexural strengthMPa | 68 ± 4 printed XY, ISO 178 (Bambu Lab); 3DXTech quotes 70[2][1] | 60.1 (ABS Pro) and 63.3 (ABS Max) printed XY, ISO 178[3][4] |
| Flexural modulusMPa | 2860 ± 130 printed XY, ISO 178 (Bambu Lab); 3DXTech quotes 4420[2][1] | 2330 (ABS Pro) and 2500 (ABS Max) printed XY, ISO 178[3][4] |
| Charpy impact, notchedkJ/m² | 4.2 ± 1.1 printed XY, ISO 179, notched (Bambu Lab)[2] | 10.5 (ABS Max) and 14.5 (ABS Pro) printed XY, ISO 179, notched[3][4] |
| Other impact data | Charpy unnotched 14.5 ± 1.5 printed XY (Bambu Lab, ISO 179)[2] | Not documented |
| Layer adhesion / Z tensileMPa | 29 ± 3 printed Z, ISO 527 (Bambu Lab)[2] | 21.9 (ABS Pro) and 25.4 (ABS Max) printed Z, ISO 527[3][4] |
| Brittleness1–5 | Brittle — snaps with little warning; notched Charpy falls from 21.5 to 4.2 kJ/m² against unfilled Bambu Lab ABS[2][21] | Tough — absorbs impact, yields before breaking[3][4] |
| Creep resistance / sustained load1–5 | Good — no creep test found; chopped glass fibre lifts modulus to 3160 MPa against 2200 for unfilled Bambu Lab ABS[2][21] | Moderate — no creep test found; Tg of 115 °C (ABS Pro) and 126 °C (ABS Max) keeps room-temperature service far below softening[3][4] |
| Fatigue / repeated-flex resistance1–5 | Below average — no S-N curve found; notched Charpy falls to 4.2 kJ/m² against 21.5 for unfilled Bambu Lab ABS[2][21] | Moderate — no S-N curve found; 6.7–7.3 % elongation and 10.5–14.5 kJ/m² notched Charpy, below unfilled Bambu Lab ABS[3][4][21] |
| Elasticity / flexibility1–5 | Rigid[2] | Rigid[3] |
| Z strength as % of XY% | 81 (Bambu Lab, printed Z against XY tensile)[2] | 63 (ABS Pro) and 71 (ABS Max), printed[3][4] |
| Thermal Properties | ||
| HDT at 0.45 MPa°C | 99 (ISO 75, 0.45 MPa, Bambu Lab) against 87 for unfilled Bambu Lab ABS[2][21] | 106.4 (ABS Pro) and 118.1 (ABS Max), ISO 75 at 0.45 MPa[3][4] |
| HDT at 1.8 MPa°C | 88 (ISO 75, 1.8 MPa, Bambu Lab) against 84 for unfilled Bambu Lab ABS[2][21] | 101.4 (ABS Pro) and 113.1 (ABS Max), ISO 75 at 1.8 MPa[3][4] |
| Glass transition (Tg)°C | Not documented | 114.9 (ABS Pro) and 126.3 (ABS Max), DSC[3][4] |
| Melting point / Vicat°C | Not documented | Amorphous — no melting point; Vicat 116.1 (ABS Pro) and 127.4 (ABS Max), ISO 306[3][4] |
| Thermal expansion (CTE)µm/m·K | Not documented | 86–89 for printed unfilled ABS (fibre Bragg grating, 25–50 °C); no grade-specific measurement published[22] |
| Environment & Chemical | ||
| UV resistance1–5 | Not documented | Months outdoors before embrittlement[16] |
| Chemical resistance | Good against weak acids, weak alkalis, oils and grease; dissolved by acetone[5] | Good against weak acids, weak alkalis, oils and grease; dissolved by acetone[5] |
| Food contact | Not food safe — Polymaker cites potential chemical leaching[16] | Not food safe — Polymaker cites potential chemical leaching[16] |
| Biodegradability / compostability | Not biodegradable[16] | Not biodegradable[16] |
| Recyclability | Mechanically recyclable but not accepted in household plastic collection[16] | Mechanically recyclable but not accepted in household plastic collection[16] |
| Health & Safety | ||
| Fume toxicity1–5 | High — hazardous VOC such as styrene; enclosure and filtration needed[23][13] | High — hazardous VOC such as styrene; enclosure and filtration needed[23][13] |
| VOC emission rateµg/min | 12–113 styrene, the dominant VOC from every ABS and HIPS combination tested[23] | 12–113 styrene, the dominant VOC from every ABS and HIPS combination tested[23] |
| Ultrafine-particle emission rateparticles/min | 2 × 10¹⁰ to 9 × 10¹⁰ median across all ABS printers, two orders of magnitude above PLA's ≈1 × 10⁸[23] | 2 × 10¹⁰ to 9 × 10¹⁰ median across all ABS printers, two orders of magnitude above PLA's ≈1 × 10⁸[23] |
| Hazardous species emitted | Styrene dominates. Bambu Lab states ABS and ASA release harmful gases such as styrene at printing temperature, which can be toxic and cause dizziness or nausea[23][13] | Styrene dominates. Bambu Lab states ABS and ASA release harmful gases such as styrene at printing temperature, which can be toxic and cause dizziness or nausea[23][13] |
| Ventilation / filtration requirement1–5 | Enclosure with carbon and HEPA filtration — an enclosure alone cut measured UFP by only about 35 %[23][13] | Enclosure with carbon and HEPA filtration — an enclosure alone cut measured UFP by only about 35 %[23][13] |
| Dust & fibre handling hazard | Glass fibre is bound in the matrix; avoid inhaling sanding dust[1] | Not documented |
| Post-Processing | ||
| Sanding & machining | Sands well and takes filler before painting[16] | Sands well and takes filler before painting[16] |
| Painting & finishing | Paints readily after light abrasion[16] | Paints readily after light abrasion[16] |
| Vapour / chemical smoothing | Not documented | Acetone vapour smoothing works[5] |
| Support material pairing | HIPS breaks away or dissolves in d-limonene; Bambu Lab sells a dedicated Support for ABS[24][13] | HIPS breaks away or dissolves in d-limonene; Bambu Lab sells a dedicated Support for ABS[24][13] |
| Dimensional accuracy & detail | Bambu Lab describes a smooth matte finish with micro-spot gloss that blurs layer lines[2] | Not documented |
| Solvents & Solubility | ||
| Soluble in | Acetone dissolves the resin and leaves the fibre as sludge; MEK, THF, ethyl acetate and chlorinated solvents do the same.[25][5] | Acetone dissolves it — the basis of ABS slurry; so do MEK, THF, ethyl acetate, chloroform, dichloromethane and toluene.[25][5] |
| Softened or crazed by | Petrol and perchloroethylene soften it and benzene attacks it; d-limonene disrupts layer adhesion in some ABS and ASA grades.[25][26] | Petrol and perchloroethylene soften it and benzene attacks it; d-limonene disrupts layer adhesion in some ABS and ASA grades.[25][26] |
| Solvent welding & smoothing agent | Acetone vapour reaches only the resin fraction, so the fibre is left standing proud of the smoothed surface.[27][5] | Acetone: about 20 min of vapour at 80 °C over 5 mm of liquid. Prusa measured layer adhesion more than doubled.[27] |
Material entries describe families or representative grades, not an interchangeable specification for every spool. Test methods, orientations and conditions may differ. Unknown values are marked “Not documented”. Prices and source dates remain historical snapshots; check the linked guide for product details. Differences highlight text, not a universal winner.
Sources for this comparison
- FibreX ABS+GF10 Glass Fiber ABS Technical Data Sheet 3DXTech · 2026-08 · tds
- Bambu Filament Technical Data Sheet V1.0 — ABS-GF Bambu Lab · 2026-08 · tds
- Polymaker ABS Pro Technical Data Sheet V1 (2026-05-29) Polymaker · 2026-05 · tds
- Polymaker ABS Max Technical Data Sheet V1.1 (2026-06-01) Polymaker · 2026-06 · tds
- PolyLite ABS Technical Data Sheet (V5.5 served at this URL) Polymaker · 2024-11 · tds
- ABS-GF — product page Bambu Lab US Store · 2026-08 · vendor
- 3DXTech product catalogue 3DXTech · 2026-08 · vendor
- Siraya Tech Fibreheart ABS-GF Filament product page Siraya Tech · 2026-08 · vendor
- SUNLU ABS-GF (ABS Glass Fiber) 3D Printer Filament 1 kg SUNLU · 2026-08 · vendor
- Polymaker product catalogue Polymaker · 2026-08 · vendor
- SUNLU E-ABS (Easy ABS) 3D Printer Filament 1 kg SUNLU · 2026-08 · vendor
- YXPOLYER ABS Enhanced product page YXPOLYER · 2026-08 · vendor
- ABS / ASA / PC Usage Guide Bambu Lab Wiki · 2026-08 · doc
- ABS — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- Max volumetric speed Prusa Knowledge Base · 2026-08 · doc
- ABS — material basics Polymaker Wiki · 2026-08 · doc
- FIBREX ABS+GF — product page (print recommendations) 3DXTech · 2026-08 · doc
- Composite materials filled with carbon, kevlar or glass Prusa Knowledge Base · 2026-08 · doc
- Filament Material Guide Prusa Knowledge Base · 2026-08 · doc
- Wet Filament — signs, causes and drying Polymaker Wiki · 2026-08 · doc
- Bambu Filament Technical Data Sheet V3.0 — ABS Bambu Lab · 2026-08 · tds
- Characterization of Thermal Expansion Coefficient of 3D Printing Polymeric Materials Using Fiber Bragg Grating Sensors Materials 17(18):4668 · 2024-09 · paper
- Emissions of Ultrafine Particles and Volatile Organic Compounds from Commercially Available Desktop Three-Dimensional Printers with Multiple Filaments (Azimi et al.) Environmental Science & Technology 50(3) 1260-1268 · 2016-01 · paper
- HIPS — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- Chemical resistance — resistance of Ensinger plastics to chemicals (DIN 50 014, 23/50) Ensinger · 2026-08 · tds
- HIPS — Knowledge Base Prusa Research · 2026-08 · doc