Filament comparison
ABS-CF vs PC-CF
Compare printing settings, strength, heat resistance, dated prices and sources.
2 selected · all documented properties
| Property | Carbon-fibre ABS (ABS-CF)ABS | Carbon-fibre PC (PC-CF)PC |
|---|---|---|
| Market snapshot | ||
| Listing priceUSD/kg; dated snapshots | $35.99/kg median; $22.00–$125.00/kg across 7 dated product listings | $62.58/kg median; $34.99–$117.33/kg across 6 dated product listings |
| Identity & Market | ||
| Base polymer / chemistry | ABS reinforced with chopped carbon fibre[1] | Polycarbonate reinforced with chopped carbon fibre[2][3] |
| Densityg/cm³ | 1.11 (ISO 1183)[1] | 1.22 (Prusament) and 1.36 (3DXTech), ISO 1183[2][3] |
| Typical priceUSD/kg | 1 kg-equivalent spools span 22–125; the middle of the market is about 36[4][5][6][7][8] | 1 kg-equivalent spools span 35–117; the middle of the market is about 63[9][10][4][11][12] |
| Price range across brandsUSD/kg | 22–125 across brands; IEMAI 22, Siraya Tech 28 and 36 for the core-shell grade, YXPOLYER 35, Push Plastic 50 at 2 kg, 3DXTech 64 at 750 g; Stratasys-compatible cartridges run far higher[4][5][6][7][13][8] | 35–117 across brands; Ambrosia 35, IEMAI 39, YXPOLYER 55, Spectrum PC CF 70, Prusament 94, 3DXTech 117[9][10][4][11][12] |
| Market availability1–5 | Available from several mainstream brands[4][5] | Available from several mainstream brands[9][4][14] |
| Spool sizes & diameters | 1.75 and 2.85 mm; 0.5, 0.75 and 2 kg spools plus Stratasys-compatible cartridges[4][5] | 1.75 and 2.85 mm; 0.75, 0.8 and 1 kg spools[9][4] |
| Typical applications | Stiff tooling and fixtures that must survive above 100 °C[1] | Stiff high-temperature structural parts — jigs, drone frames and under-bonnet brackets[2][3] |
| Diameter tolerance± mm | Not documented | ±0.04 (Prusament PC Blend Carbon Fiber)[2] |
| Printing Parameters | ||
| Nozzle temperature°C | Not documented | 285 ± 10 (Prusament)[2] |
| Bed temperature°C | Not documented | 110 ± 10 (Prusament)[2] |
| Enclosure / chamber requirement1–5 | Enclosure recommended[15] | Enclosure required (passive)[2][15] |
| Part cooling fan | Not documented | Off — Prusa allows 0–20 % and warns cooling significantly reduces interlayer adhesion[2] |
| Bed surface & adhesion aid | Clean the plate and apply glue; Simplify3D also lists Kapton tape and ABS slurry[15][16] | PEI with a glue stick or a commercial adhesive[17] |
| Warping tendency1–5 | Moderate — needs adhesion aid or draught shield; the fibre reduces warping against unfilled ABS[15] | High — enclosure needed for reliable large parts; the fibre reduces warping against unfilled PC[2][15] |
| Bed-adhesion difficulty1–5 | Needs a specific surface plus adhesive[15] | Needs a specific surface plus adhesive[17][18] |
| Stringing / oozing tendency1–5 | Slight — Polymaker advises 1–2 mm retraction at 20–30 mm/s[19] | Moderate — retraction tuning needed; Polymaker flags stringing as a common PC problem[18] |
| Overall printing difficulty1–5 | Intermediate — dry filament and a tuned profile; hardened nozzle mandatory[15] | Advanced — enclosure, hardware upgrades, tuning; hardened nozzle mandatory[15][2] |
| Hardware Wear & Reliability | ||
| Nozzle hardness required1–4 | Hardened steel required[15] | Hardened steel required[15] |
| Abrasiveness1–5 | Highly abrasive — standard CF composite[15] | Highly abrasive — standard CF composite[15] |
| Nozzle clog risk1–5 | Moderate — needs dry filament and a clean nozzle; 3DXTech specifies a hardened nozzle of 0.4 mm minimum and 0.25 mm layers or higher, and Prusa lists composites as a higher clogging risk[20][21][22] | High — jams from moisture, heat creep or particles; PC already absorbs water from the air and 3DXTech adds a hardened 0.4 mm minimum nozzle, 0.25 mm layers and a 120 °C pre-dry[23][17][21] |
| Heat-creep / jam sensitivity1–5 | Slightly sensitive[16] | Slightly sensitive[17] |
| Hotend requirement | No special hot-end required[16] | All-metal hot end required (Simplify3D)[17] |
| Moisture Behaviour | ||
| Moisture absorption (hygroscopicity)1–5 | Moderate — the ABS matrix takes up 0.51–0.65 % saturated at 25 °C / 55 % RH and 3DXTech specifies a 80 °C, 4 h pre-dry[24][25][20] | Low (0.1–0.3 %) — the PC matrix takes up 0.15–0.25 % and 3DXTech specifies a 120 °C, 4 h pre-dry[26][27][23] |
| Equilibrium moisture content at ~50 % RH% | Not documented | 0.11 after 7 days at 24 °C / 22 % RH (Prusa Polymers)[2] |
| Symptoms when wet | Bubbling and popping at the nozzle, stringing and a rough surface[28] | Bubbling and popping at the nozzle, stringing and a rough surface[28] |
| Effect of moisture on strength | Polymaker rates ABS moderate-sensitivity and publishes no dry-versus-conditioned figures; absorbed water flashes to steam in the hotend and shows as bubbling and poor layer adhesion[28] | No dry-versus-conditioned figures are published. Polymaker calls PC highly hygroscopic and requires a 70–80 °C dry for 6–8 h; run wet, the loss shows as surface defects and poor layer adhesion[18][28] |
| Storage requirement | Sealed with desiccant; Polymaker rates ABS moderate-sensitivity[28] | Airtight containers with desiccant to prevent reabsorption[18] |
| Mechanical Properties | ||
| Tensile strength (XY)MPa | 46 at break (printed XY, ISO 527)[1] | 64 ± 3 printed horizontal and 70 ± 3 printed vertical at yield, ISO 527-1 (Prusament); 3DXTech quotes 73 at break[2][3] |
| Young's modulusMPa | 5210 (printed XY, ISO 527) — more than double unfilled ABS[1] | 2600 printed horizontal and 3200 printed vertical, ISO 527-1 (Prusament); 3DXTech quotes 6980[2][3] |
| Elongation at break% | 2 at break (printed XY, ISO 527)[1] | 4.6 at yield printed horizontal (Prusament); 3DXTech quotes 2.1 at break[2][3] |
| Flexural strengthMPa | 76 (printed XY, ISO 178)[1] | 94 ± 3 printed horizontal and 130 ± 2 printed vertical, ISO 178 (Prusament); 3DXTech quotes 85[2][3] |
| Flexural modulusMPa | 5260 (printed XY, ISO 178)[1] | 3500 printed horizontal and 4200 printed vertical, ISO 178 (Prusament); 3DXTech quotes 6540[2][3] |
| Charpy impact, notchedkJ/m² | Not documented | 12 ± 1 printed horizontal and 17 ± 2 printed vertical, ISO 179-1 notched (Prusament)[2] |
| Other impact data | Not documented | Charpy unnotched 32 ± 5 printed horizontal and 35 ± 4 printed vertical (Prusament, ISO 179-1)[2] |
| Layer adhesion / Z tensileMPa | Not documented | 23 ± 2 (Prusa Polymers interlayer adhesion test) — above the 21 ± 2 of unfilled Prusament PC Blend[2][27] |
| Brittleness1–5 | Brittle — snaps with little warning; elongation at break 2 %[1] | Moderate[2][3] |
| Hardness (scale-specific)Shore A / Shore D / Rockwell | Not documented | 83 Shore D (Prusa Polymers method), against 79 for unfilled Prusament PC Blend[2][27] |
| Creep resistance / sustained load1–5 | Good — no creep test found; chopped carbon fibre restrains matrix flow and modulus rises to 5210 MPa against 2200–2330 for unfilled ABS[1][24][25] | Excellent — holds load for years. Room-temperature tensile creep of moulded unfilled PC ran unbroken at 41 MPa until the test was stopped; short carbon fibre raises the flexural modulus from about 2.1 to 3.5-6.5 GPa, which reduces creep strain further[29][2] |
| Fatigue / repeated-flex resistance1–5 | Below average — no S-N curve found; elongation at break falls to 2 % against 10.5 % for unfilled ABS[1][24] | Good. No fatigue test data was found for a carbon-fibre PC filament; the unfilled polymer is rated Good on the same scale[29] |
| Elasticity / flexibility1–5 | Rigid[1] | Rigid[2] |
| Thermal Properties | ||
| HDT at 0.45 MPa°C | Not documented | 114 (ISO 75, 0.45 MPa, Prusament)[2] |
| HDT at 1.8 MPa°C | Not documented | 106 (ISO 75, 1.8 MPa, Prusament), against 93 for unfilled Prusament PC Blend[2][27] |
| Glass transition (Tg)°C | 105 (DSC)[1] | 127 (3DXTech, DSC)[3] |
| Continuous service temperature°C | Not documented | 113 — Prusa publishes this as the temperature resistance of Prusament PC Blend[27] |
| Thermal expansion (CTE)µm/m·K | 19–25 along the print bead and 80–84 in the build direction at 30 °C (20 wt% CF, large-format printed, TMA)[30] | Not documented |
| Environment & Chemical | ||
| UV resistance1–5 | Not documented | Degrades within weeks outdoors unless stabilised[18] |
| Chemical resistance | Good against weak acids, weak alkalis, oils and grease; dissolved by acetone[31] | Withstands oils, solvents and fuels; Polymaker rates it good against weak acids[18] |
| Food contact | Not food safe — Polymaker cites potential chemical leaching[19] | Bisphenol-A polycarbonate is not offered as food-contact filament[18] |
| Biodegradability / compostability | Not biodegradable[19] | Not biodegradable[18] |
| Recyclability | Mechanically recyclable but not accepted in household plastic collection[19] | Mechanically recyclable but not accepted in household plastic collection[18] |
| Electrical & ESD properties | Surface resistance above 10⁹ ohm/sq — not static-dissipative (ASTM D257)[1] | Surface resistance above 10⁹ ohm/sq — not static-dissipative (3DXTech, ASTM D257)[3] |
| Health & Safety | ||
| Fume toxicity1–5 | High — hazardous VOC such as styrene; enclosure and filtration needed[32][15] | Moderate — measurable VOCs and UFPs, ventilation advised[32] |
| VOC emission rateµg/min | 12–113 styrene, the dominant VOC from every ABS and HIPS combination tested[32] | Not documented |
| Ultrafine-particle emission rateparticles/min | 2 × 10¹⁰ to 9 × 10¹⁰ median across all ABS printers, two orders of magnitude above PLA's ≈1 × 10⁸[32] | ≈4 × 10¹⁰ median — the highest ultrafine-particle rate of the nine filaments in the chamber study, above every ABS tested[32] |
| Hazardous species emitted | Styrene dominates. Bambu Lab states ABS and ASA release harmful gases such as styrene at printing temperature, which can be toxic and cause dizziness or nausea[32][15] | Not documented |
| Ventilation / filtration requirement1–5 | Enclosure with carbon and HEPA filtration — an enclosure alone cut measured UFP by only about 35 %[32][15] | Ventilated room or enclosure recommended[32][15] |
| Dust & fibre handling hazard | Carbon fibre is bound in the matrix; sanding dust should not be inhaled[1] | Carbon fibre is bound in the matrix; sanding dust should not be inhaled[3] |
| Post-Processing | ||
| Sanding & machining | Sands well and takes filler before painting[19] | Sands and machines well; the toughness means it cuts rather than chips[17] |
| Painting & finishing | Paints readily after light abrasion[19] | Not documented |
| Gluing & solvent welding | Not documented | Cyanoacrylate; dichloromethane solvent-welds PC but is a laboratory reagent[17] |
| Vapour / chemical smoothing | Acetone smoothing is blunted by the fibre — only the resin fraction dissolves[31] | No practical vapour smoothing[17] |
| Support material pairing | HIPS breaks away or dissolves in d-limonene; Bambu Lab sells a dedicated Support for ABS[33][15] | Prints its own supports; 3DXTech sells a dedicated PC break-away support[17] |
| Solvents & Solubility | ||
| Soluble in | Acetone dissolves the resin and leaves the fibre as sludge; MEK, THF, ethyl acetate and chlorinated solvents do the same.[34][31] | Dichloromethane and chloroform dissolve the matrix and leave the fibre; DMF and dioxane do the same (Covestro).[35] |
| Softened or crazed by | Petrol and perchloroethylene soften it and benzene attacks it; d-limonene disrupts layer adhesion in some ABS and ASA grades.[34][36] | Methanol, butyl acetate, ether, 1 % NaOH and phthalate plasticisers stress-crack it; acetone, MEK and xylene swell it.[35] |
| Solvent welding & smoothing agent | Acetone vapour reaches only the resin fraction, so the fibre is left standing proud of the smoothed surface.[37][31] | Dichloromethane cement welds the resin, but the fibre keeps the joint from flowing closed. Controlled carcinogen.[38] |
Material entries describe families or representative grades, not an interchangeable specification for every spool. Test methods, orientations and conditions may differ. Unknown values are marked “Not documented”. Prices and source dates remain historical snapshots; check the linked guide for product details. Differences highlight text, not a universal winner.
Sources for this comparison
- CarbonX Carbon Fiber ABS Technical Data Sheet 3DXTech · 2026-08 · tds
- Prusament PC Blend Carbon Fiber Technical Datasheet v2.0 Prusa Polymers · 2023-04 · tds
- CarbonX Carbon Fiber ezPC Polycarbonate Technical Data Sheet 3DXTech · 2026-08 · tds
- 3DXTech product catalogue 3DXTech · 2026-08 · vendor
- Push Plastic product catalogue Push Plastic · 2026-08 · vendor
- IEMAI CF-ABS 3D Printing Filament product page IEMAI 3D · 2026-08 · vendor
- Siraya Tech Fibreheart ABS-CF Filament product page Siraya Tech · 2026-08 · vendor
- YXPOLYER ABS CF product page YXPOLYER · 2026-08 · vendor
- Printed Solid product catalogue Printed Solid · 2026-08 · vendor
- Spectrum PC CF Carbon Black, 1.75 mm / 250 g 3DJAKE · 2026-08 · vendor
- IEMAI CF-PC 3D Printing Filament product page IEMAI 3D · 2026-08 · vendor
- YXPOLYER PC CF product page YXPOLYER · 2026-08 · vendor
- Siraya Tech Fibreheart ABS-CF Core Filament product page Siraya Tech · 2026-08 · vendor
- Filastruder product catalogue Filastruder · 2026-08 · vendor
- ABS / ASA / PC Usage Guide Bambu Lab Wiki · 2026-08 · doc
- ABS — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- Polycarbonate — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- PC — material basics Polymaker Wiki · 2026-08 · doc
- ABS — material basics Polymaker Wiki · 2026-08 · doc
- CARBONX ABS+CF — product page (print recommendations) 3DXTech · 2026-08 · doc
- Composite materials filled with carbon, kevlar or glass Prusa Knowledge Base · 2026-08 · doc
- Carbon Fiber Filled — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- CARBONX ezPC+CF — product page (print recommendations) 3DXTech · 2026-08 · doc
- Bambu Filament Technical Data Sheet V3.0 — ABS Bambu Lab · 2026-08 · tds
- Polymaker ABS Pro Technical Data Sheet V1 (2026-05-29) Polymaker · 2026-05 · tds
- Bambu Filament Technical Data Sheet V2.0 — PC Bambu Lab · 2026-08 · tds
- Prusament PC Blend Technical Datasheet v1.1 Prusa Polymers · 2022-02 · tds
- Wet Filament — signs, causes and drying Polymaker Wiki · 2026-08 · doc
- Experimental data for creep and dynamic mechanical properties of polycarbonate and polycarbonate/ABS Data in Brief 42:108264 · 2022-06 · paper
- Effects of Fiber Orientation on the Coefficient of Thermal Expansion of Fiber-Filled Polymer Systems in Large Format Polymer Extrusion-Based Additive Manufacturing Materials 15(8):2764 · 2022-04 · paper
- PolyLite ABS Technical Data Sheet (V5.5 served at this URL) Polymaker · 2024-11 · tds
- Emissions of Ultrafine Particles and Volatile Organic Compounds from Commercially Available Desktop Three-Dimensional Printers with Multiple Filaments (Azimi et al.) Environmental Science & Technology 50(3) 1260-1268 · 2016-01 · paper
- HIPS — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- Chemical resistance — resistance of Ensinger plastics to chemicals (DIN 50 014, 23/50) Ensinger · 2026-08 · tds
- Makrolon — The chemical resistance (Makrolon 2800, 6 days at 23 °C and 50 °C) Covestro · 2016-12 · tds
- HIPS — Knowledge Base Prusa Research · 2026-08 · doc
- Improve your 3D prints with chemical smoothing Prusa Research · 2026-08 · doc
- Weld-On 3 Acrylic Plastic Cement — technical data sheet (shipped as dichloromethane) IPS Corporation · 2002-07 · tds