2 selected · all documented properties
| Property | Silk PLAPLA | TPU 85AFLEX |
|---|---|---|
| Market snapshot | ||
| Listing priceUSD/kg; dated snapshots | $19.49/kg median; $9.75–$24.99/kg across 15 dated product listings | $89.89/kg median; $31.99–$106.05/kg across 6 dated product listings |
| Identity & Market | ||
| Base polymer / chemistry | PLA with a gloss-forming additive package; suppliers publish the composition as polylactic acid only[1] | Soft thermoplastic polyurethane at 82–85 Shore A[2][3][4] |
| Densityg/cm³ | 1.27 (ISO 1183)[1] | 1.11 (BASF Ultrafuse 85A) to 1.19 (NinjaFlex 85A), ISO 1183 / ASTM D792[4][2] |
| Typical priceUSD/kg | Mainstream 1 kg spools cluster near 20[5][6][7] | 1 kg-equivalent spools span 32–106; the middle of the market is about 90[8][9][2] |
| Price range across brandsUSD/kg | 10–25 across brands; CHCKX 10 in a 16-roll bundle, SUNLU 13, LANDU 18, YXPOLYER 20, Polymaker 22, Devil Design 25[10][11][12][13][14] | 32–106 across brands; Siraya Tech Flex TPU 85A 32 at 1 kg, add:north TPU Pro Matte 85A 72, Recreus Filaflex 82A 90 at 500 g, Proto-pasta Clear Flexible TPU 90, 3DXTech 3DXFLEX 85A 96, NinjaTek NinjaFlex 106[15][8][9][16][2] |
| Market availability1–5 | Stocked by most mainstream brands[5][10][17] | Available from several mainstream brands[8][15] |
| Spool sizes & diameters | 1.75 mm; 1 and 1.1 kg spools; dual- and tri-colour coextruded variants[18][19] | 1.75, 2.85 and 3 mm; 0.5, 1 and 2 kg spools[8][15][2] |
| Typical applications | Decorative prints where surface gloss matters more than strength[1] | Soft-touch grips, seals, wearables and anything that must compress and rebound[2][3] |
| Diameter tolerance± mm | ±0.03 (Bambu Lab)[20] | Not documented |
| Printing Parameters | ||
| Nozzle temperature°C | 210–240 — 20 °C above the plain PLA window[1] | 200–220 (BASF Ultrafuse 85A, 210 typical)[4] |
| Bed temperature°C | 35–45[1] | 40 (BASF Ultrafuse 85A)[4] |
| Enclosure / chamber requirement1–5 | Open frame is fine[1][21] | Open frame is fine[4] |
| Part cooling fan | Fan on[1] | Not documented |
| Bed surface & adhesion aid | Cool Plate SuperTack, smooth PEI or textured PEI[1] | PEI sheet or painter's tape; Polymaker warns TPU can over-stick and advises a glue stick as a release agent[22][23] |
| Maximum volumetric flow (mm³/s; see test conditions)mm³/s | Not documented | 1.2–3.2 at the 15–40 mm/s BASF specifies on a 0.4 mm nozzle at 0.2 mm layer[4] |
| Warping tendency1–5 | None[1] | None[4] |
| Bed-adhesion difficulty1–5 | Sticks to anything[24] | Sticks to anything — Recreus states its 82A grade has excellent bed adhesion without a heated bed or additives[3] |
| Stringing / oozing tendency1–5 | Not documented | High — drying plus tuning needed[25][23] |
| Overall printing difficulty1–5 | Easy — minor profile tuning; hotter nozzle and slower cap of 250 mm/s[1] | Advanced — enclosure, hardware upgrades, tuning; at this hardness the filament will not push through a Bowden tube[2][3] |
| Extruder requirement | Not documented | Direct drive only. NinjaTek calls its 85A grade ideal for direct-drive extruders and Recreus specifies direct-drive printers for 82A; BASF caps print speed at 15–40 mm/s with a nozzle of 0.4 mm or larger[2][3][4] |
| Hardware Wear & Reliability | ||
| Nozzle hardness required1–4 | Brass fine indefinitely[21] | Brass fine indefinitely[26] |
| Abrasiveness1–5 | Non-abrasive[27][21] | Non-abrasive[26] |
| Nozzle clog risk1–5 | Very low[21] | High — jams from moisture, heat creep or particles[25][23] |
| Heat-creep / jam sensitivity1–5 | Moderate — good heatbreak cooling needed; PLA softens below 60 °C[28] | Very high — softens in the cold zone readily; soft filament buckles between the drive gear and the melt zone[23][2] |
| Hotend requirement | No special hot-end required[24] | No special hot-end required, but a direct-drive extruder is (Simplify3D)[22] |
| Moisture Behaviour | ||
| Moisture absorption (hygroscopicity)1–5 | Moderate — 0.40 % saturated at 25 °C / 55 % RH[1] | Moderate — NinjaTek measures 0.22 % in 24 h (ASTM D570) and BASF specifies a 70 °C dry for at least 5 h[2][4] |
| Equilibrium moisture content at ~50 % RH% | 0.40 saturated at 25 °C / 55 % RH (Bambu Lab)[1] | 0.22 after 24 h water immersion (NinjaFlex 85A, ASTM D570) — an immersion figure, not an equilibrium moisture content at 50 % RH[2] |
| Drying temperature & time | 55 °C for 8 h in a forced-air dryer, or 65–75 °C for 12 h on an X1 heatbed[1][29] | 70 °C for at least 5 h in a hot-air dryer or vacuum oven (BASF)[4] |
| Symptoms when wet | Bubbling and popping at the nozzle, stringing, rough surface and weak layers[25] | Bubbling and popping at the nozzle, stringing and a rough surface[25] |
| Effect of moisture on strength | Polymaker rates PLA low-sensitivity — the loss shows as poor layer adhesion and brittle layers rather than a published strength figure[25] | Polymaker groups TPU with the highly hygroscopic materials; wet TPU prints with poor layer adhesion and weak, brittle layers[25] |
| Storage requirement | Sealed with desiccant below 20 % RH; shelf life at ambient is long[30][24] | Sealed with desiccant; often kept in a dryer during the print[25] |
| Mechanical Properties | ||
| Tensile strength (XY)MPa | 33 (printed XY, ISO 527); eSun Silk broke 22 % below the 16-brand PLA mean on identical 4×4 mm bars[1][31] | 26 ultimate (NinjaFlex 85A, ASTM D638)[2] |
| Young's modulusMPa | 2130 (printed XY, ISO 527)[1] | 12 (NinjaFlex 85A, ASTM D638) — two orders of magnitude below any rigid filament; NinjaTek's 95A Cheetah reaches 26 by the same method[2][32] |
| Elongation at break% | 2.8 (printed XY, ISO 527) — a quarter of PLA Basic at 12.2[1][30] | 650 at break (Filaflex 82A) and 660 (NinjaFlex 85A); BASF measures 600 in XY and 320 in ZX[3][2][4] |
| Flexural strengthMPa | 75 (printed XY, ISO 178)[1] | Not documented |
| Flexural modulusMPa | 2460 (printed XY, ISO 178)[1] | Not documented |
| Charpy impact, notchedkJ/m² | 10.3 (printed XY, ISO 179, notched); unnotched 18.5[1] | Not documented |
| Layer adhesion / Z tensileMPa | 25 (printed Z, ISO 527), and flexural Z collapses to 30 against 75 in XY; eSun Silk broke at 12.3 kg where twelve of the 16 plain PLAs managed 44.6–61.5 kg[1][31][33] | Not documented |
| Brittleness1–5 | Brittle — snaps with little warning[1] | Very ductile — bends far before failing[2] |
| Hardness (scale-specific)Shore A / Shore D / Rockwell | Not documented | 29 Shore D / 85 Shore A (BASF Ultrafuse 85A, ISO 7619-1); 85 Shore A (NinjaFlex, ASTM D2240); 82 A nominal for Filaflex[2][4][3] |
| Creep resistance / sustained load1–5 | Poor — no silk-specific creep data published; plain PLA sagged from 12 to 18.7–20.3 mm over 5 days at 1.25 kg[34][35] | Poor — no 85A creep test; a printed 95A TPU bar crept from 74.5 to 82.7 mm over 5 days at 1.25 kg, and softer grades creep more[36] |
| Fatigue / repeated-flex resistance1–5 | Poor — no grade-specific S-N curve; plain printed PLA ran 38 000–49 000 cycles at 30 % of tensile strength (R = 0.2)[37][28] | Excellent — living hinges viable[23] |
| Elasticity / flexibility1–5 | Rigid[1] | Rubbery / highly elastic[2][3] |
| Z strength as % of XY% | 76 by tensile, 40 by flexural (printed, Bambu Lab)[1] | 53 — BASF measures 320 % elongation at break in ZX against 600 % in XY[4] |
| Wear resistance & friction | Not documented | Abrasion 0.08 g mass loss over 10 000 cycles (NinjaFlex, ASTM D4060); 82 mm³ (BASF, ISO 4649)[2][4] |
| Thermal Properties | ||
| HDT at 0.45 MPa°C | 60 (ISO 75, 0.45 MPa)[1] | Not documented |
| HDT at 1.8 MPa°C | 56 (ISO 75, 1.8 MPa)[1] | Not documented |
| Glass transition (Tg)°C | 57 (DSC)[1] | Not documented |
| Melting point / Vicat°C | 158 peak melt (DSC); Vicat 66 °C[1] | 216 melting (NinjaFlex 85A, DSC)[2] |
| Continuous service temperature°C | 50 — a loaded bar begins to move at this temperature (My Tech Fun, eSun eSilk PLA)[33] | Not documented |
| Annealing response | 50–55 °C for 6–12 h[1] | Not documented |
| Flammability / UL 94 | Flammable; no UL 94 rating published by the major brands[30][38] | Not documented |
| Environment & Chemical | ||
| UV resistance1–5 | Degrades within weeks outdoors[28][39] | Good — years with some colour shift; Polymaker lists UV exposure among the conditions TPU withstands[23] |
| Chemical resistance | Good against weak acids, oils and grease; poor against strong acids and alkalis; dissolved by chloroform, THF and hot benzene[38][28] | Withstands industrial solvents and UV exposure (Polymaker)[23] |
| Water / humidity resistance in service1–5 | Good — insoluble in water[30] | Not documented |
| Food contact | Base resin is food-contact grade, but printed layer grooves harbour bacteria; Prusa advises against food use[28] | Not food safe without specific certification (Polymaker)[23] |
| Biodegradability / compostability | Industrially compostable only — needs sustained 55 °C; not home compostable[40][28] | Not biodegradable[23] |
| Recyclability | Mechanically recyclable; not accepted in household plastic collection[40] | Not accepted in household plastic collection[23] |
| Health & Safety | ||
| Fume toxicity1–5 | Low hazard — minimal VOC and particle emission[41] | Low hazard — minimal VOC and particle emission; TPU was not among the nine filaments in the chamber study[41] |
| Ventilation / filtration requirement1–5 | None needed in a normal room[41] | Open a window / occasional ventilation[41] |
| Post-Processing | ||
| Sanding & machining | Wet sanding — dry sanding heats the surface by friction and smears it[39][28] | Difficult to sand or smooth; Polymaker limits post-processing to trimming or tumbling[23] |
| Gluing & solvent welding | Cyanoacrylate for most joints; some grades partially dissolve and bond with acetone[28][42] | Cyanoacrylate bonds TPU; no common solvent welds it[23] |
| Vapour / chemical smoothing | No practical vapour smoothing — only chloroform, hot benzene or THF, which are laboratory-only[28] | No practical vapour smoothing[23] |
| Support material pairing | Support for PLA (Bambu Lab)[1] | Polymaker warns TPU supports are often very difficult to remove[23] |
| Dimensional accuracy & detail | 55° overhangs and 30 mm bridges; gloss hides fine detail and is destroyed by sanding[1] | Not documented |
| Solvents & Solubility | ||
| Soluble in | Chloroform: 10 % w/v in 2–4 h at 23 °C, every grade and morphology; THF and DMF only at 65 °C. Laboratory reagents.[43] | DMF, DMSO, NMP and THF dissolve TPU; acetone, MEK and cyclohexanone are partial solvents. All laboratory reagents.[44] |
| Softened or crazed by | Acetone, ethyl acetate and toluene plasticise it but dissolve <1 % even at 65 °C; submersion in acetone crazes and destroys parts.[43][45] | Toluene and benzene swell it up to +50 % by weight at 23 °C; esters swell it severely; ethanol and IPA soften it.[44] |
| Solvent welding & smoothing agent | Chloroform vapour smooths and welds PLA at the cost of tensile strength; acetone does not smooth it at all.[46][45] | None practical — the true solvents (DMF, THF, NMP) are laboratory reagents and leave the joint swollen and weak.[44] |
Material entries describe families or representative grades, not an interchangeable specification for every spool. Test methods, orientations and conditions may differ. Unknown values are marked “Not documented”. Prices and source dates remain historical snapshots; check the linked guide for product details. Differences highlight text, not a universal winner.
Sources for this comparison
- Bambu Filament Technical Data Sheet V1.0 — PLA Silk+ Bambu Lab · 2026-08 · tds
- NinjaFlex 85A Technical Specifications NinjaTek · 2026-08 · tds
- Filaflex 82A product page (Shore hardness and elongation) Recreus · 2026-08 · vendor
- Ultrafuse TPU 85A Technical Data Sheet (Version 3.0) BASF Forward AM · 2022-08 · tds
- Panchroma Silk PLA collection Polymaker Shop · 2026-08 · vendor
- Spectrum PLA Silk — product listing 3DJake International · 2026-08 · vendor
- 3DJake ecoPLA Silk Black 1.75mm 1000g 3DJake International · 2026-08 · vendor
- 3DXTech product catalogue 3DXTech · 2026-08 · vendor
- Siraya Tech Flex TPU 85A Filament — product page Siraya Tech · 2026-08 · vendor
- Sunlu Silk PLA+ 1.75mm 1kg Sunlu Official Store · 2026-08 · vendor
- Bambu Lab PLA Silk 1.75mm 1kg 3D Universe · 2026-08 · vendor
- CHCKX 16 Pack Silk Dual Color PLA Filament Bundle CHCKX (Amazon US) · 2026-08 · vendor
- YXPOLYER Silk PLA Black&Gold product page YXPOLYER · 2026-08 · vendor
- LANDU Silk Tri-Color PLA Filament 1.75 mm 1 kg LANDU (Amazon US) · 2026-08 · vendor
- Proto-pasta product catalogue Proto-pasta · 2026-08 · vendor
- add:north TPU Pro Matte 85A product page add:north · 2026-08 · vendor
- Overture Silk PLA 1.75mm Overture3D · 2026-08 · vendor
- eSUN PLA-Silk Magic 1.75mm eSUN Official Store · 2026-08 · vendor
- JAYO Silk PLA+ 1.75mm 1.1kg JAYO Official Store · 2026-08 · vendor
- PLA Basic — product page Bambu Lab US Store · 2026-08 · vendor
- Filament Material Guide Prusa Knowledge Base · 2026-08 · doc
- Flexible (TPE/TPU) — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- TPU — material basics Polymaker Wiki · 2026-08 · doc
- PLA — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- Wet Filament — signs, causes and drying Polymaker Wiki · 2026-08 · doc
- Extrudr Product Catalogue (DURAPRO PA12 data block) Extrudr · 2025-03 · tds
- Prusament PLA — material page Prusa Polymers · 2026-08 · doc
- PLA — material guide Prusa Knowledge Base · 2026-08 · doc
- Filament Drying Recommendations Bambu Lab Wiki · 2026-08 · doc
- Bambu Filament Technical Data Sheet V3.0 — PLA Basic Bambu Lab · 2026-08 · tds
- 16 PLA brand comparison test — results spreadsheet My Tech Fun (Igor Gaspar) · 2022-10 · test
- NinjaTek technical specs comparison chart (Cheetah, NinjaFlex, Armadillo, Alloy 910, Nylon 645) NinjaTek · 2026-08 · tds
- Testing eSun PLA filaments: PLA-ST vs PLA+ vs Silk PLA My Tech Fun (Igor Gaspar) · 2026-08 · test
- BambuLab PLA Basic vs PLA Tough vs PLA-CF — results spreadsheet My Tech Fun (Igor Gaspar) · 2026-08 · test
- PolyTerra PLA vs PLA+ — results spreadsheet My Tech Fun (Igor Gaspar) · 2026-08 · test
- BambuLab TPU 95A HF vs Qidi TPU 95A HF — results spreadsheet My Tech Fun (Igor Gaspar) · 2024-02 · test
- Mechanical Properties of Additively Manufactured Polymeric Materials — PLA and PETG — For Biomechanical Applications Polymers 16(13):1868 · 2024-06 · paper
- PolyLite PLA Technical Data Sheet V5.4 Polymaker · 2024-11 · tds
- Prusament PLA Technical Data Sheet v1.0 Prusa Polymers · 2018-09 · tds
- Filamentive PLA (recycled) — product page Filamentive · 2026-08 · vendor
- Emissions of Ultrafine Particles and Volatile Organic Compounds from Commercially Available Desktop Three-Dimensional Printers with Multiple Filaments (Azimi et al.) Environmental Science & Technology 50(3) 1260-1268 · 2016-01 · paper
- Prusament rPLA Corn Pigment 1kg — product page Prusa Research · 2026-08 · vendor
- Solubility Study of Ingeo Biopolymer Grades in Common Organic Solvents (NWPD003) NatureWorks · 2019-10 · tds
- Elastollan — Chemical properties: swelling and chemical resistance BASF · 2026-08 · tds
- Improve your 3D prints with chemical smoothing Prusa Research · 2026-08 · doc
- Effect of vapour smoothing in trichloromethane on 3D printed PLA — surface, mechanical and chemical structure Pitale, Keche & Chopra, Engineering Research Express 6(4) 045579 · 2024-12 · paper