Filament comparison
rPLA vs PP-GF
Compare printing settings, strength, heat resistance, dated prices and sources.
2 selected · all documented properties
| Property | Recycled PLA (rPLA)PLA | Glass-fibre PP (PP-GF)POLYOLEFIN |
|---|---|---|
| Market snapshot | ||
| Listing priceUSD/kg; dated snapshots | $20.79/kg median; $16.05–$40.64/kg across 8 dated product listings | $49.09/kg median; $46.27–$86.01/kg across 3 dated product listings |
| Identity & Market | ||
| Base polymer / chemistry | PLA regranulated from post-industrial PLA manufacturing waste; post-consumer feedstock is rare[1][2][3] | Polypropylene reinforced with chopped glass fibre[4][5] |
| Densityg/cm³ | 1.24 (ISO 1183)[1] | 1.12 (Prusament PP Glass Fiber, ISO 1183) — the glass lifts it above water[4] |
| Typical priceUSD/kg | 1 kg spools run 20–22[6][7][8] | 1 kg-equivalent spools cluster near 49[9][10][11] |
| Price range across brandsUSD/kg | 16–41 across brands; Fiberlogy refill 16, Filamentive 750 g 41[12][13] | 46-86 across brands; BCN3D PP GF30 46 at 700 g, BASF Ultrafuse PP GF30 49 at 2.2 kg, Prusament PP Glass Fiber 86 at 850 g[9][10][11] |
| Market availability1–5 | Available from several mainstream brands[2][3][8] | Available from several mainstream brands[9][10][11] |
| Spool sizes & diameters | 1.75 and 2.85 mm; 0.75, 0.85 and 1 kg spools plus spool-less refills[14][12][2] | 1.75 and 2.85 mm; 700 g, 850 g and 2.2 kg spools[9][10][11] |
| Typical applications | General-purpose printing where the feedstock's recycled content matters more than an exact colour match[2][3] | Stiff, chemically resistant parts where PP-CF's cost or conductivity is unwanted[5] |
| Diameter tolerance± mm | ±0.03 guaranteed by Prusa Research today; the 2021 datasheet specified ±0.05, against ±0.02 for virgin Prusament PLA[2][1][15] | ±0.04 (Prusament)[4] |
| Printing Parameters | ||
| Nozzle temperature°C | 210 ± 10 (Prusament); 200 ± 15 (Filamentive)[1][3] | 245 ± 10 (Prusament) — 25 °C below the carbon-fibre grade[4][16] |
| Bed temperature°C | 40–60 (Prusament); up to 60 (Filamentive)[1][3] | 95 ± 10 (Prusament)[4] |
| Enclosure / chamber requirement1–5 | Open frame is fine[1][17] | Enclosure recommended — Simplify3D lists an enclosure as a hardware requirement and Polymaker advises one below 70 °C ambient to stop warping and cracking[18][19] |
| Part cooling fan | 100 %[1] | Off — Prusa runs 0 % except 100 % on bridges[4] |
| Maximum volumetric flow (mm³/s; see test conditions)mm³/s | Not documented | 4 at Prusa's 50 mm/s cap on a 0.4 mm nozzle at 0.2 mm layer[4][20] |
| Warping tendency1–5 | None — brim not generally needed[1] | High — enclosure needed for reliable large parts; Prusa recommends a brim[4] |
| Bed-adhesion difficulty1–5 | Sticks to anything[21] | Very difficult — special plates or slurry required[4] |
| Overall printing difficulty1–5 | Beginner — prints on any machine out of the box[1][17] | Advanced — enclosure, hardware upgrades, tuning; hardened nozzle mandatory[4] |
| Extruder requirement | Not documented | Prusa states a hardened nozzle is necessary and recommends a brim[4] |
| Hardware Wear & Reliability | ||
| Nozzle hardness required1–4 | Brass fine indefinitely[17] | Hardened steel required[4] |
| Abrasiveness1–5 | Non-abrasive[22][17] | Highly abrasive — standard GF composite[4] |
| Nozzle clog risk1–5 | Very low[17] | Moderate — needs dry filament and a clean nozzle; Prusa lists higher risk of nozzle clogging for glass-filled composites[23] |
| Heat-creep / jam sensitivity1–5 | Moderate — good heatbreak cooling needed; PLA softens below 60 °C[24] | Not documented |
| Hotend requirement | No special hot-end required[21] | Not documented |
| Moisture Behaviour | ||
| Moisture absorption (hygroscopicity)1–5 | Moderate — 0.3 % after both 24 h and 7 days at 28 °C / 37 % RH (Prusa Polymers method), against 0.19 % in 7 days for virgin Prusament PLA[1][15] | Low (0.1–0.3 %) — 0.11 % at both 24 h and 7 days, higher than the carbon-fibre grade's 0.04 % but still very low[4][16] |
| Equilibrium moisture content at ~50 % RH% | 0.3 after 24 h and 7 days at 28 °C / 37 % RH (Prusa Polymers method)[1] | 0.11 after 24 h and 0.11 after 7 days at 24 °C / 22 % RH (Prusa Polymers)[4] |
| Symptoms when wet | Bubbling and popping at the nozzle, stringing, rough surface and weak layers[25] | Not documented |
| Effect of moisture on strength | Polymaker rates PLA low-sensitivity — the loss shows as poor layer adhesion and brittle layers rather than a published strength figure[25] | Not applicable in practice at 0.11 % equilibrium uptake[4] |
| Storage requirement | Sealed with desiccant below 20 % RH; shelf life at ambient is long[26][21] | No special storage needed[4] |
| Mechanical Properties | ||
| Tensile strength (XY)MPa | 49 printed horizontal and 55 printed vertical XZ (ISO 527-1, yield); virgin Prusament PLA gives 51 and 59 by the same method[1][15] | 46.6 ± 1.3 filament tensile yield (Prusament, ISO 527) — more than double the carbon-fibre grade's 21[4][16] |
| Young's modulusMPa | 2100 printed horizontal, 2300 printed vertical XZ (ISO 527-1); virgin Prusament PLA 2300 and 2400[1][15] | Not documented |
| Elongation at break% | 3.1 at yield printed horizontal (ISO 527-1); virgin Prusament PLA 2.9[1][15] | Not documented |
| Flexural strengthMPa | 82 printed horizontal, 87 printed vertical XZ (ISO 178); virgin Prusament PLA 83 and 99[1][15] | Not documented |
| Flexural modulusMPa | 3100 printed horizontal (ISO 178) — the same as virgin Prusament PLA[1][15] | Not documented |
| Charpy impact, notchedkJ/m² | Not documented | 7.9 ± 0.4 printed horizontal and 9.9 ± 0.8 printed vertical XZ (ISO 179-1, notched)[4] |
| Other impact data | Charpy unnotched 14.0 printed horizontal (ISO 179-1); virgin Prusament PLA 13[1][15] | Not documented |
| Layer adhesion / Z tensileMPa | 21 ± 2 (Prusa Polymers interlayer adhesion test); virgin Prusament PLA 17 ± 3 by the same test[1][15] | Not documented |
| Brittleness1–5 | Brittle — snaps with little warning[24][22] | Moderate[4] |
| Hardness (scale-specific)Shore A / Shore D / Rockwell | 80 Shore D (Prusa Polymers in-house method); virgin Prusament PLA 81[1][15] | Rockwell R102 (and M95) on extruded unfilled PP stock (ASTM D785); no figure is published for a glass-fibre PP filament[27] |
| Creep resistance / sustained load1–5 | Poor — no recycled-PLA creep data published; virgin PLA sagged from 12 to 18.7–20.3 mm over 5 days at 1.25 kg[28][29] | Not documented |
| Fatigue / repeated-flex resistance1–5 | Poor — no grade-specific S-N curve; plain printed PLA ran 38 000–49 000 cycles at 30 % of tensile strength (R = 0.2)[30][24] | Not documented |
| Elasticity / flexibility1–5 | Rigid[22] | Rigid[4] |
| Thermal Properties | ||
| HDT at 0.45 MPa°C | 55 (ISO 75, 0.45 MPa) — the same as virgin Prusament PLA[1][15] | 138.3 (ISO 75, 0.45 MPa)[4] |
| HDT at 1.8 MPa°C | 53 (ISO 75, 1.8 MPa); virgin Prusament PLA 55[1][15] | 112.6 (ISO 75, 1.8 MPa)[4] |
| Continuous service temperature°C | 55 (Filamentive states heat resistance up to 55 °C)[3] | Not documented |
| Thermal expansion (CTE)µm/m·K | 96–99 for plain printed PLA (fibre Bragg grating, 25–50 °C); no grade-specific measurement published[31] | Not documented |
| Flammability / UL 94 | Flammable; no UL 94 rating published by the major brands[26][32] | Not documented |
| Environment & Chemical | ||
| UV resistance1–5 | Degrades within weeks outdoors[24][33] | Not documented |
| Chemical resistance | Good against weak acids, oils and grease; poor against strong acids and alkalis; dissolved by chloroform, THF and hot benzene[32][24] | Excellent against acids, alkalis and most solvents[19] |
| Water / humidity resistance in service1–5 | Good — insoluble in water[26] | Excellent — essentially unaffected[4] |
| Food contact | Filamentive certifies its rPLA to EN 71-3 and lists it food safe; printed layer grooves still harbour bacteria[3][24] | Not documented |
| Biodegradability / compostability | Industrially compostable only — needs sustained 55 °C; not home compostable[3] | Not documented |
| Recyclability | The feedstock itself; Filamentive uses 50 % post-industrial content and runs a PLA take-back scheme[3][13] | Not documented |
| Health & Safety | ||
| Fume toxicity1–5 | Low hazard — minimal VOC and particle emission[34] | Low hazard — minimal VOC and particle emission. Inferred: no polyolefin was among the nine filaments in the Azimi chamber study, so this is a family-level judgement rather than a measurement[34] |
| Hazardous species emitted | Prusament rPLA Corn Pigment uses organic waste pigments such as red algae, which give a noticeable scent while printing[2] | Not documented |
| Ventilation / filtration requirement1–5 | None needed in a normal room[34] | Open a window / occasional ventilation. Inferred — no polyolefin was measured in the chamber study[34] |
| Dust & fibre handling hazard | Not documented | Glass fibre is bound in the matrix; avoid inhaling sanding dust[4] |
| Post-Processing | ||
| Sanding & machining | Wet sanding — dry sanding heats the surface by friction and smears it[33][24] | Not documented |
| Gluing & solvent welding | Superglue for most joints; acetone works on some grades depending on additives and colour[2] | Not documented |
| Vapour / chemical smoothing | No practical vapour smoothing — only chloroform, hot benzene or THF, which are laboratory-only[24] | Not documented |
| Solvents & Solubility | ||
| Soluble in | Chloroform: 10 % w/v in 2–4 h at 23 °C, every grade and morphology; THF and DMF only at 65 °C. Laboratory reagents.[35] | None at room temperature; chloroform dissolves the matrix at 60 °C and xylene at about 118 °C, leaving the fibre.[36][37] |
| Softened or crazed by | Acetone, ethyl acetate and toluene plasticise it but dissolve <1 % even at 65 °C; submersion in acetone crazes and destroys parts.[35][38] | Xylene, decalin, CCl4 and chlorobenzene are heavily absorbed at 20 °C; oleum, chlorosulphonic acid and bromine destroy it.[36] |
| Solvent welding & smoothing agent | Chloroform vapour smooths and welds PLA at the cost of tensile strength; acetone does not smooth it at all.[39][38] | None — nothing softens PP at room temperature, so joints have to be welded thermally rather than chemically.[36] |
Material entries describe families or representative grades, not an interchangeable specification for every spool. Test methods, orientations and conditions may differ. Unknown values are marked “Not documented”. Prices and source dates remain historical snapshots; check the linked guide for product details. Differences highlight text, not a universal winner.
Sources for this comparison
- Prusament PLA Recycled Technical Datasheet v1.0 Prusa Polymers · 2021-12 · tds
- Prusament rPLA Corn Pigment 1kg — product page Prusa Research · 2026-08 · vendor
- Filamentive PLA (recycled) — product page Filamentive · 2026-08 · vendor
- Prusament PP Glass Fiber Technical Datasheet v1.0 Prusa Polymers · 2024-11 · tds
- Prusament PP Glass Fiber — material page Prusa Polymers · 2026-08 · doc
- 3D-Fuel ReFuel Recycled PLA 1kg 3D-Fuel · 2026-08 · vendor
- Proto-pasta Black Recycled PLA 1kg Proto-pasta · 2026-08 · vendor
- Formfutura ReForm rPLA (White) 1kg Filament2Print · 2026-08 · vendor
- BASF Ultrafuse PP GF30 Black 2.85 mm 2.200 g igo3d · 2026-08 · vendor
- BCN3D PP GF30 Black 2.85 mm 700 g igo3d · 2026-08 · vendor
- Prusa Prusament PP Glass Fiber Natural (NFC), 1.75 mm / 850 g 3DJAKE · 2026-08 · vendor
- Fiberlogy rPLA Refill Anthracite 850 g 3DJake International · 2026-08 · vendor
- Filamentive PLA (rPLA) 750 g CREATE Education · 2026-08 · vendor
- Kimya PLA-R 750 g Crea3D · 2026-08 · vendor
- Prusament PLA Technical Datasheet v1.1 Prusa Polymers · 2022-02 · tds
- Prusament PP Carbon Fiber Technical Datasheet v1.0 Prusa Polymers · 2024-11 · tds
- Filament Material Guide Prusa Knowledge Base · 2026-08 · doc
- Polypropylene — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- PP — material basics Polymaker Wiki · 2026-08 · doc
- Max volumetric speed Prusa Knowledge Base · 2026-08 · doc
- PLA — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- Prusament PLA — material page Prusa Polymers · 2026-08 · doc
- Composite materials filled with carbon, kevlar or glass Prusa Knowledge Base · 2026-08 · doc
- PLA — material guide Prusa Knowledge Base · 2026-08 · doc
- Wet Filament — signs, causes and drying Polymaker Wiki · 2026-08 · doc
- Bambu Filament Technical Data Sheet V3.0 — PLA Basic Bambu Lab · 2026-08 · tds
- TECAFINE PP natural — stock shape properties Ensinger · 2026-08 · tds
- BambuLab PLA Basic vs PLA Tough vs PLA-CF — results spreadsheet My Tech Fun (Igor Gaspar) · 2026-08 · test
- PolyTerra PLA vs PLA+ — results spreadsheet My Tech Fun (Igor Gaspar) · 2026-08 · test
- Mechanical Properties of Additively Manufactured Polymeric Materials — PLA and PETG — For Biomechanical Applications Polymers 16(13):1868 · 2024-06 · paper
- Characterization of Thermal Expansion Coefficient of 3D Printing Polymeric Materials Using Fiber Bragg Grating Sensors Materials 17(18):4668 · 2024-09 · paper
- PolyLite PLA Technical Data Sheet V5.4 Polymaker · 2024-11 · tds
- Prusament PLA Technical Data Sheet v1.0 Prusa Polymers · 2018-09 · tds
- Emissions of Ultrafine Particles and Volatile Organic Compounds from Commercially Available Desktop Three-Dimensional Printers with Multiple Filaments (Azimi et al.) Environmental Science & Technology 50(3) 1260-1268 · 2016-01 · paper
- Solubility Study of Ingeo Biopolymer Grades in Common Organic Solvents (NWPD003) NatureWorks · 2019-10 · tds
- Pro-fax and Moplen polypropylene — Chemical Resistance Guide (20, 60 and 100 °C) LyondellBasell · 2026-08 · tds
- US 5,278,282 Polymer recycling by selective dissolution — xylene dissolution temperatures Nauman & Lynch, Rensselaer Polytechnic Institute · 1994-01 · paper
- Improve your 3D prints with chemical smoothing Prusa Research · 2026-08 · doc
- Effect of vapour smoothing in trichloromethane on 3D printed PLA — surface, mechanical and chemical structure Pitale, Keche & Chopra, Engineering Research Express 6(4) 045579 · 2024-12 · paper