| Property | High-Speed PLAPLA | Polypropylene (PP)POLYOLEFIN |
|---|---|---|
| Market snapshot | ||
| Listing priceUSD/kg; dated snapshots | $19.99/kg median; $11.49–$32.99/kg across 10 dated product listings | $46.56/kg median; $31.99–$53.00/kg across 4 dated product listings |
| Identity & Market | ||
| Base polymer / chemistry | PLA with rheology and crystallisation tuned for high volumetric flow; melt index 15.4 g/10 min vs 7–11 for standard PLA[1][2] | Polypropylene — a semi-crystalline polyolefin with no polar groups, so it neither absorbs water nor bonds to most bed surfaces[3][4] |
| Densityg/cm³ | 1.23 (ISO 1183, at 21.5 °C)[1] | 0.91 (Prusa PP composite, ISO 1183) — the lightest common filament[5] |
| Typical priceUSD/kg | Mainstream 1 kg spools cluster near 20[6][7][8] | 1 kg-equivalent spools span 27–53; the middle of the market is about 44[9][10][11][12] |
| Price range across brandsUSD/kg | 11–33 across brands; budget house brands 11–18, Prusament 33[13][14][15] | 27–53 across brands; Reli3D 32 on Amazon, SUNLU 44 at 0.8 kg, Fiberlogy 49 at 750 g, IEMAI 3D 53, and the 3DJake PP listing spans 27–49[9][16][10][11][12] |
| Market availability1–5 | Stocked by most mainstream brands[17][8][18] | Available from several mainstream brands[16][10][9] |
| Spool sizes & diameters | 1.75 mm; 1 kg spools[6][8] | 1.75 and 2.85 mm; 0.75 kg spools are common[10] |
| Typical applications | Large or repetitive prints on printers that can sustain high flow[19][17] | Living hinges, chemical-resistant containers, automotive clips and packaging prototypes[3] |
| Diameter tolerance± mm | ±0.03 (Bambu Lab PLA Basic, rated to 258 mm/s)[20] | Not documented |
| Printing Parameters | ||
| Nozzle temperature°C | 210–230 for high-speed work; 190–210 at classic speeds[1][17] | 210–230 (Braskem-type PE/PP window); Formfutura's Centaur PP melts at 205 ± 15 °C[3] |
| Bed temperature°C | 30–60 (Polymaker); 35–45 (Bambu Lab)[1][21] | Not documented |
| Enclosure / chamber requirement1–5 | Open frame is fine[1] | Enclosure recommended — Simplify3D lists an enclosure as a hardware requirement and Polymaker advises one below 70 °C ambient to stop warping and cracking[22][4] |
| Part cooling fan | Fan on[1] | Part cooling fan required (Simplify3D)[22] |
| Bed surface & adhesion aid | Not documented | Packing tape, a polypropylene sheet, or a PP-specific adhesive such as Magigoo PP — ordinary PLA and ABS adhesives do not hold it[22][4] |
| Maximum volumetric flow (mm³/s; see test conditions)mm³/s | ≈24 at 300 mm/s with a 0.4 mm nozzle and 0.2 mm layer; 30 % more flow than regular PLA at the same temperature[1][17][19][23] | Not documented |
| Warping tendency1–5 | None[1] | High — enclosure needed for reliable large parts; PP's crystallinity drives shrinkage and Prusa recommends a brim on its PP grades[5][24] |
| Bed-adhesion difficulty1–5 | Sticks to anything[25] | Very difficult — special plates or slurry required. PP bonds to almost nothing; a polypropylene-specific tape or adhesive is the normal answer[5][4] |
| Stringing / oozing tendency1–5 | Not documented | Slight — Polymaker advises 1–2 mm retraction at 20–30 mm/s[4] |
| Overall printing difficulty1–5 | Easy — minor profile tuning; needs a printer that can actually reach the flow rate[17][1] | Advanced — enclosure, hardware upgrades, tuning; bed adhesion is the whole problem[4][5] |
| Hardware Wear & Reliability | ||
| Nozzle hardness required1–4 | Brass fine indefinitely[26] | Brass fine indefinitely for unfilled grades — Simplify3D states no special hotend is required[22] |
| Abrasiveness1–5 | Non-abrasive[27][26] | Non-abrasive when unfilled[22] |
| Nozzle clog risk1–5 | Very low[26] | Low — Simplify3D lists no special hotend requirement for PP and clogging is not among its listed drawbacks[28][22] |
| Heat-creep / jam sensitivity1–5 | Moderate — good heatbreak cooling needed; PLA softens below 60 °C[29] | Slightly sensitive[22] |
| Hotend requirement | No special hot-end required[25] | No special hot-end required (Simplify3D)[22] |
| Moisture Behaviour | ||
| Moisture absorption (hygroscopicity)1–5 | Moderate — 0.40 % equilibrium at 23 °C / 70 % RH[1] | Negligible (<0.1 % EMC) — Prusa measures 0.03 % in 24 h and 0.04 % in 7 days on its PP composite, the lowest figures it publishes for any filament[5] |
| Equilibrium moisture content at ~50 % RH% | 0.40 equilibrium at 23 °C / 70 % RH (Polymaker PolySonic)[1] | 0.03 after 24 h and 0.04 after 7 days at 24 °C / 22 % RH (Prusa Polymers, measured on its PP composite)[5] |
| Drying temperature & time | 55 °C for 6 h; 50 °C for 8 h (Bambu Lab)[1][21] | No drying step is published for PP; uptake is below the level that affects printing[5] |
| Symptoms when wet | Bubbling and popping at the nozzle, stringing, rough surface and weak layers[28] | Bubbling and popping at the nozzle; Polymaker still advises a 70 °C dry for 4–6 h despite the low uptake[4] |
| Effect of moisture on strength | Polymaker rates PLA low-sensitivity — the loss shows as poor layer adhesion and brittle layers rather than a published strength figure[28] | Not applicable in practice — with equilibrium uptake at 0.04 %, there is no moisture-driven strength loss to measure. Polymaker's sensitivity tiers put polyolefins below even PLA[5][28] |
| Storage requirement | Sealed with desiccant below 20 % RH; shelf life at ambient is long[21][25] | No special storage needed[5] |
| Mechanical Properties | ||
| Tensile strength (XY)MPa | 43.9 at 300 mm/s and 46.0 at 46.7 mm/s (printed XY, ISO 527); 58.6 on My Tech Fun bars for Creality Hyper PLA[1][30] | 12 at yield (Formfutura Centaur PP, ASTM D638)[3] |
| Young's modulusMPa | 2650 at 300 mm/s, 2878 at classic speed (printed XY, ISO 527)[1] | 724 on extruded PP stock (ASTM D638; converted from 105,000 psi)[31] |
| Elongation at break% | 15.1 at 300 mm/s, 21.5 at classic speed (printed XY, ISO 527)[1] | Above 600 at break (Formfutura Centaur PP, ASTM D638)[3] |
| Flexural strengthMPa | 71.4 at 300 mm/s, 76.5 at classic speed (printed XY, ISO 178)[1] | 31.0 on extruded PP stock (ASTM D790; converted from 4500 psi)[31] |
| Flexural modulusMPa | 2798 at 300 mm/s, 2868 at classic speed (printed XY, ISO 178)[1] | 402 flexural modulus (Formfutura Centaur PP, ASTM D790) — an order of magnitude below any rigid filament[3] |
| Charpy impact, notchedkJ/m² | 5.0 at 300 mm/s, 6.1 at classic speed (printed XY, ISO 179, notched)[1] | Not documented |
| Other impact data | Printing at 300 mm/s instead of 46.7 mm/s costs 4.6 % tensile strength and 18 % notched Charpy[1] | Izod notched 112 J/m on extruded PP stock, converted from 2.1 ft-lb/in (ASTM D256)[31] |
| Layer adhesion / Z tensileMPa | 32.4 at 300 mm/s, 37.3 at classic speed (printed Z, ISO 527); 35.3 for Creality Hyper PLA vs 23.0 for average PLA on identical bars[1][30] | Not documented |
| Brittleness1–5 | Moderate[1] | Very ductile — bends far before failing[3] |
| Hardness (scale-specific)Shore A / Shore D / Rockwell | 78.7 Shore D measured on printed bars for Sunlu PLA Meta (My Tech Fun), against 75.3 for the same maker's plain PLA[32] | Rockwell R102 (and M95) on extruded PP stock (ASTM D785)[31] |
| Creep resistance / sustained load1–5 | Poor — 12 mm bar sagged to 17.7 mm over 6 days at 1.25 kg[30] | Below average[3] |
| Fatigue / repeated-flex resistance1–5 | Poor — no grade-specific S-N curve; plain printed PLA ran 38 000–49 000 cycles at 30 % of tensile strength (R = 0.2)[33][29] | Excellent — living hinges viable, the classic polypropylene application[3] |
| Elasticity / flexibility1–5 | Rigid[1] | Semi-flexible[3] |
| Z strength as % of XY% | 74 at 300 mm/s, 81 at classic speed (printed)[1] | Not documented |
| Thermal Properties | ||
| HDT at 0.45 MPa°C | 53 (ISO 75, 0.45 MPa)[1] | 74 on extruded PP stock (ASTM D648 at 66 psi; converted from 165 °F)[31] |
| HDT at 1.8 MPa°C | 52 (ISO 75, 1.8 MPa)[1] | Not documented |
| Glass transition (Tg)°C | 59 (DSC)[1] | Not documented |
| Melting point / Vicat°C | 164 peak melt (DSC); crystallisation 96 °C, Vicat 61 °C[1] | 205 ± 15 melting (Formfutura Centaur PP)[3] |
| Continuous service temperature°C | 53 — loaded bars begin to move at this temperature[30] | Bounded by a melting point of 205 ± 15 °C and by the 158 °C heat deflection of the carbon-filled grade; no loaded-bar service figure is published for unfilled PP[3][5] |
| Thermal expansion (CTE)µm/m·K | 96–99 for plain printed PLA (fibre Bragg grating, 25–50 °C); no grade-specific measurement published[34] | Not documented |
| Flammability / UL 94 | Flammable; no UL 94 rating published by the major brands[21][2] | Flammable; no UL 94 rating published for the grades surveyed[5] |
| Environment & Chemical | ||
| UV resistance1–5 | Degrades within weeks outdoors[29][35] | Months outdoors before embrittlement — unstabilised polypropylene chalks under UV[4] |
| Chemical resistance | Good against weak acids, oils and grease; poor against strong acids and alkalis[1] | Excellent against acids, alkalis and most solvents — the usual reason to choose PP[4] |
| Water / humidity resistance in service1–5 | Good — insoluble in water[21] | Excellent — essentially unaffected[5] |
| Food contact | Base resin is food-contact grade, but printed layer grooves harbour bacteria; Prusa advises against food use[29] | Polypropylene is a common food-packaging polymer, but no filament here carries a food-contact certification[4] |
| Biodegradability / compostability | Industrially compostable only — needs sustained 55 °C; not home compostable[36][29] | Not biodegradable[4] |
| Recyclability | Mechanically recyclable; not accepted in household plastic collection[36] | Mechanically recyclable as resin code 5, but printed waste is not accepted in household collection[4] |
| Health & Safety | ||
| Fume toxicity1–5 | Low hazard — minimal VOC and particle emission[37] | Low hazard — minimal VOC and particle emission. Inferred: no polyolefin was among the nine filaments in the Azimi chamber study, so this is a family-level judgement rather than a measurement[37] |
| Ventilation / filtration requirement1–5 | None needed in a normal room[37] | Open a window / occasional ventilation. Inferred — no polyolefin was measured in the chamber study[37] |
| Post-Processing | ||
| Sanding & machining | Wet sanding — dry sanding heats the surface by friction and smears it[35][29] | Sands poorly — the waxy surface loads abrasive paper[22] |
| Painting & finishing | Not documented | Paint and adhesives do not key to untreated PP; flame or plasma treatment is normally needed first[4] |
| Gluing & solvent welding | Cyanoacrylate for most joints; some grades partially dissolve and bond with acetone[29][38] | Nothing common bonds untreated PP; flame or plasma treatment is needed before adhesives key[4] |
| Vapour / chemical smoothing | No practical vapour smoothing — only chloroform, hot benzene or THF, which are laboratory-only[29] | No practical vapour smoothing[22] |
| Support material pairing | PolySupport and PolyDissolve S1 (Polymaker)[1] | Prints its own supports; no soluble support is rated for PP[22] |
| Dimensional accuracy & detail | Not documented | Shrinkage and warping dominate; the low modulus means parts flex rather than hold tolerance[5] |
| Solvents & Solubility | ||
| Soluble in | Chloroform: 10 % w/v in 2–4 h at 23 °C, every grade and morphology; THF and DMF only at 65 °C. Laboratory reagents.[39] | None at room temperature; chloroform dissolves it at 60 °C and xylene at about 118 °C — the xylene-solubles route.[40][41] |
| Softened or crazed by | Acetone, ethyl acetate and toluene plasticise it but dissolve <1 % even at 65 °C; submersion in acetone crazes and destroys parts.[39][42] | Xylene, decalin, CCl4 and chlorobenzene are heavily absorbed at 20 °C; oleum, chlorosulphonic acid and bromine destroy it.[40] |
| Solvent welding & smoothing agent | Chloroform vapour smooths and welds PLA at the cost of tensile strength; acetone does not smooth it at all.[43][42] | None — nothing softens PP at room temperature, so joints have to be welded thermally rather than chemically.[40] |
Material entries describe families or representative grades, not an interchangeable specification for every spool. Test methods, orientations and conditions may differ. Unknown values are marked “Not documented”. Prices and source dates remain historical snapshots; check the linked guide for product details. Differences highlight text, not a universal winner.
Sources for this comparison
- PolySonic PLA Technical Data Sheet V5.4 Polymaker · 2024-11 · tds
- PolyLite PLA Technical Data Sheet V5.4 Polymaker · 2024-11 · tds
- Centaur PP Technical Data Sheet Formfutura · 2026-08 · tds
- PP — material basics Polymaker Wiki · 2026-08 · doc
- Prusament PP Carbon Fiber Technical Datasheet v1.0 Prusa Polymers · 2024-11 · tds
- PolySonic PLA 1.75mm/1kg — product page Polymaker Shop · 2026-08 · vendor
- Overture High Speed PLA 1.75mm Overture3D · 2026-08 · vendor
- High Speed PLA filament collection Anycubic Official Store · 2026-08 · vendor
- SUNLU product catalogue SUNLU · 2026-08 · vendor
- Fiberlogy PP Natural — product page 3DJake International · 2026-08 · vendor
- Reli3D Low Warp PP Filament 1.75 mm 1 kg Black — Amazon listing Amazon.com · 2026-08 · vendor
- IEMAI 3D PP 3D Printing Filament — store page IEMAI 3D · 2026-08 · vendor
- PLA Meta filament collection Sunlu Official Store · 2026-08 · vendor
- QIDI PLA Rapido 1.75mm 1kg 3D Printers Depot · 2026-08 · vendor
- Prusament PLA Prusa Pro Green 1kg (NFC) Prusa Research · 2026-08 · vendor
- PP filament listing 3DJake International · 2026-08 · vendor
- PolySonic PLA — product page Polymaker · 2026-08 · vendor
- Creality PLA filament collection Creality Official Store · 2026-08 · vendor
- Polymaker Launches New High-Speed 3D Printing Filament — PolySonic PLA & PLA Pro Polymaker · 2023-11 · doc
- PLA Basic — product page Bambu Lab US Store · 2026-08 · vendor
- Bambu Filament Technical Data Sheet V3.0 — PLA Basic Bambu Lab · 2026-08 · tds
- Polypropylene — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- Max volumetric speed Prusa Knowledge Base · 2026-08 · doc
- Prusament PP Glass Fiber Technical Datasheet v1.0 Prusa Polymers · 2024-11 · tds
- PLA — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- Filament Material Guide Prusa Knowledge Base · 2026-08 · doc
- Prusament PLA — material page Prusa Polymers · 2026-08 · doc
- Wet Filament — signs, causes and drying Polymaker Wiki · 2026-08 · doc
- PLA — material guide Prusa Knowledge Base · 2026-08 · doc
- Creality Hyper PLA filament review — results spreadsheet My Tech Fun (Igor Gaspar) · 2026-08 · test
- TECAFINE PP natural — stock shape properties Ensinger · 2026-08 · tds
- Carbon Fiber PLA vs META-PLA vs PLA+ vs PLA by Sunlu — results spreadsheet My Tech Fun (Igor Gaspar) · 2026-08 · test
- Mechanical Properties of Additively Manufactured Polymeric Materials — PLA and PETG — For Biomechanical Applications Polymers 16(13):1868 · 2024-06 · paper
- Characterization of Thermal Expansion Coefficient of 3D Printing Polymeric Materials Using Fiber Bragg Grating Sensors Materials 17(18):4668 · 2024-09 · paper
- Prusament PLA Technical Data Sheet v1.0 Prusa Polymers · 2018-09 · tds
- Filamentive PLA (recycled) — product page Filamentive · 2026-08 · vendor
- Emissions of Ultrafine Particles and Volatile Organic Compounds from Commercially Available Desktop Three-Dimensional Printers with Multiple Filaments (Azimi et al.) Environmental Science & Technology 50(3) 1260-1268 · 2016-01 · paper
- Prusament rPLA Corn Pigment 1kg — product page Prusa Research · 2026-08 · vendor
- Solubility Study of Ingeo Biopolymer Grades in Common Organic Solvents (NWPD003) NatureWorks · 2019-10 · tds
- Pro-fax and Moplen polypropylene — Chemical Resistance Guide (20, 60 and 100 °C) LyondellBasell · 2026-08 · tds
- US 5,278,282 Polymer recycling by selective dissolution — xylene dissolution temperatures Nauman & Lynch, Rensselaer Polytechnic Institute · 1994-01 · paper
- Improve your 3D prints with chemical smoothing Prusa Research · 2026-08 · doc
- Effect of vapour smoothing in trichloromethane on 3D printed PLA — surface, mechanical and chemical structure Pitale, Keche & Chopra, Engineering Research Express 6(4) 045579 · 2024-12 · paper