Filament comparison
PEBA vs PEEK
Compare printing settings, strength, heat resistance, dated prices and sources.
2 selected · all documented properties
| Property | PEBA (polyether block amide)FLEX | PEEKHIGHTEMP |
|---|---|---|
| Market snapshot | ||
| Listing priceUSD/kg; dated snapshots | $60.99/kg median; $60.99–$60.99/kg across 1 dated product listings | $531.87/kg median; $296.14–$770.00/kg across 5 dated product listings |
| Identity & Market | ||
| Base polymer / chemistry | Polyether block amide: rigid polyamide and flexible polyether blocks.[1] | Polyether ether ketone — a semi-crystalline polyaryletherketone[2] |
| Densityg/cm³ | 1.01 g/cm³ (GB/T 1033; eSUN manufacturer data)[1] | 1.30 (ISO 1183)[2][3] |
| Typical priceUSD/kg | Not documented | 1 kg-equivalent spools span 296–770; the middle of the market is about 532[4][5][6] |
| Price range across brandsUSD/kg | Not documented | 296-770 across brands and spool sizes; 3D4Makers recycled R-PEEK 296 at 750 g, IEMAI 3D 420 at 1 kg, LEHVOSS Luvocom 3F PEEK 9581 532 at 2 kg, 3DXTech ThermaX PEEK 770 at 500 g[4][5][6] |
| Market availability1–5 | Not documented | Niche, a handful of specialist brands[4][5][3] |
| Spool sizes & diameters | 1.75 mm diameter, 1 kg spool.[7] | 1.75 and 2.85 mm; 200 g to 2 kg spools[4][5][3] |
| Typical applications | Manufacturer applications include footwear, sports equipment and cushioning.[1] | Aerospace brackets, semiconductor handling, sterilisable medical tooling and downhole parts[2] |
| Printing Parameters | ||
| Nozzle temperature°C | 230–260 °C; 240 °C recommended.[1] | 380-400 (3DXTech printed-specimen conditions); Victrex quotes a 340-450 melt range for AM 450 FIL[2][3] |
| Bed temperature°C | 60–90 °C[1] | 130–140 (3DXTech)[2] |
| Enclosure / chamber requirement1–5 | Not documented | Actively heated chamber required[8][9] |
| Recommended chamber temperature°C | Not documented | Not less than 150 for semi-crystalline printing (Victrex AM 450 FIL); bed above 150[3] |
| Part cooling fan | 10–50% fan recommended; mechanical-test specimens used 50–100%.[1] | Not documented |
| Bed surface & adhesion aid | PEI build plate[1] | Not documented |
| Maximum volumetric flow (mm³/s; see test conditions)mm³/s | 9 mm³/s maximum in eSUN spiral-vase test; mechanical specimens used 2 mm³/s. Linear recommendation 25–110 mm/s is a separate quantity.[1] | Not documented |
| Warping tendency1–5 | Not documented | Severe — heated chamber needed[8] |
| Bed-adhesion difficulty1–5 | Not documented | Very difficult — special plates or slurry required[8] |
| Overall printing difficulty1–5 | Not documented | Expert / industrial hardware only[8][9] |
| Extruder requirement | Not documented | An all-metal hot end rated above 400 °C and a heated chamber; 3DXTech tests at 0.25 mm layer height on a 0.4 mm nozzle[2][8] |
| Hardware Wear & Reliability | ||
| Nozzle hardness required1–4 | Not documented | Brass fine indefinitely for unfilled grades, but brass softens near these nozzle temperatures — hardened or plated hot ends are the norm[8] |
| Abrasiveness1–5 | Not documented | Non-abrasive when unfilled[2] |
| Nozzle clog risk1–5 | Not documented | Moderate — needs dry filament and a clean nozzle; 3DXTech lists no special nozzle concerns but a mandatory 120 °C pre-dry before every print[10] |
| Moisture Behaviour | ||
| Equilibrium moisture content at ~50 % RH% | Not documented | 0.45 at saturation, 23 °C (ISO 62); 0.55 at 100 °C[3] |
| Drying temperature & time | 70–75 °C for 6–8 h; re-dry after receiving or extended exposure.[1] | 120 °C for 5 h, target below 0.020 % moisture (Victrex AM 450 FIL)[3] |
| Effect of moisture on strength | Not documented | No dry-versus-conditioned figures are published; 3DXTech mandates a 120 °C, 4 h pre-dry before every print because trapped water flashes to steam at these nozzle temperatures[10] |
| Mechanical Properties | ||
| Tensile strength (XY)MPa | >16.5 MPa printed XY, GB/T 1040; manufacturer lower bound, not an exact measurement.[1] | 60-100 (printed XY): Victrex AM 450 FIL 60-80 at yield and 3DXTech 100, both ISO 527; 98 at yield injection-moulded[2][3] |
| Young's modulusMPa | Not documented | 3000-4000 (printed XY, ISO 527, Victrex AM 450 FIL); 3720 (3DXTech); 4000 injection-moulded[2][3] |
| Elongation at break% | >520% printed XY, GB/T 1040; manufacturer lower bound.[1] | 28 (printed XY, ISO 527) — remarkably ductile for a high-temperature polymer[2] |
| Flexural strengthMPa | Not documented | 130 (printed XY, ISO 178)[2] |
| Flexural modulusMPa | Not documented | 2700 (printed XY, ISO 178)[2] |
| Charpy impact, notchedkJ/m² | Not documented | 6.0 (injection-moulded, ISO 179/1eA); unnotched does not break[3] |
| Other impact data | Not documented | Izod notched 7.0 kJ/m2 injection-moulded (ISO 180/A). Printed anisotropy is extreme: VICTREX AM 200 on a Stratasys F900 gives Izod notched 1380-1530 J/m XZ against 30-62 J/m ZX (ASTM D256)[3][11] |
| Layer adhesion / Z tensileMPa | 7.5 MPa printed Z, GB/T 1040 (manufacturer test)[1] | 20-85 at yield (printed ZX, ISO 527, Victrex AM 450 FIL); the spread is set by chamber temperature and weld quality[3] |
| Brittleness1–5 | Not documented | Tough — absorbs impact, yields before breaking[2] |
| Hardness (scale-specific)Shore A / Shore D / Rockwell | 90 Shore A nominal grade designation; do not compare numerically with Shore D or Rockwell.[7] | Shore D 84.5 (injection-moulded, ISO 868); Rockwell M100 / R125 on extruded PEEK stock (ASTM D785)[3][12] |
| Creep resistance / sustained load1–5 | Not documented | Excellent — holds load for years. Victrex rates PEEK for long-term creep; injection-moulded flexural stress at 3.5 % strain falls only from 125 MPa at 23 °C to 85 MPa at 125 °C, and extruded stock is rated to 249 °C continuous[13][3][12] |
| Fatigue / repeated-flex resistance1–5 | Not documented | Excellent — living hinges viable. Victrex rates PEEK for long-term fatigue as well as creep[13] |
| Elasticity / flexibility1–5 | Not documented | Rigid[2] |
| Z strength as % of XY% | Not documented | 71-84 (VICTREX AM 200 LMPAEK printed on the Stratasys F900 and Fortus 450mc, ZX against XZ tensile yield, ASTM D638); unfilled PEEK's own ZX spread is wider[11] |
| Thermal Properties | ||
| HDT at 0.45 MPa°C | Not documented | 140 (printed XY, ISO 75 at 0.45 MPa, 3DXTech)[2] |
| HDT at 1.8 MPa°C | Not documented | 152 (unannealed, ISO 75-2/Af, Victrex AM 450 FIL); 160 on extruded stock (ASTM D648 at 264 psi)[3][12] |
| Glass transition (Tg)°C | Not documented | 143 (DSC, 3DXTech); Victrex gives onset 143 and midpoint 150 (ISO 11357-2)[2][3] |
| Melting point / Vicat°C | 110 °C Vicat softening (GB/T 1633, 120 °C/h, 10 N); not HDT or a continuous-use rating.[1] | 343 melting (ISO 11357-3, Victrex); VICTREX AM 200 LMPAEK melts at 303[3][11] |
| Continuous service temperature°C | Not documented | 240 UL 746B relative thermal index, strength (RTI electrical 260, impact 180); Ensinger rates extruded PEEK stock at 249 long term[3][12] |
| Thermal expansion (CTE)µm/m·K | Not documented | 37.8 (extruded PEEK stock, 23-60 °C, ASTM E831; source states 2.1e-5 in/in/°F), rising to 41.9 at 60-100 °C and 55.8 at 100-150 °C[12] |
| Flammability / UL 94 | Not documented | UL 94 V-0 at 1.5 mm on the base resin; glow-wire flammability index 960 °C at 2.0 mm (IEC 60695-2-12)[2][3] |
| Environment & Chemical | ||
| Chemical resistance | Not documented | Outstanding — resistant to almost all solvents and to steam sterilisation[2] |
| Water / humidity resistance in service1–5 | Not documented | Excellent — essentially unaffected; 0.45 % water at saturation and resistant to steam sterilisation[3][2] |
| Health & Safety | ||
| Fume toxicity1–5 | Not documented | Moderate — measurable VOCs and UFPs, ventilation advised. None of these polymers was in the chamber study, and all are processed far above the temperatures it covered[14] |
| Ventilation / filtration requirement1–5 | Not documented | Ventilated room or enclosure recommended[14] |
| Solvents & Solubility | ||
| Soluble in | Not documented | 95–98 wt% sulphuric acid dissolves it — 10 g per 100 mL at 40–70 °C gives a dark red solution. Laboratory route only.[15][16] |
| Softened or crazed by | Not documented | Concentrated nitric, hydrofluoric, hydrobromic and hydriodic acids attack it; DCM, DMSO and THF swell thin-walled sections.[17][16] |
| Solvent welding & smoothing agent | Not documented | None — no solvent softens PEEK, so parts are joined thermally or mechanically, never chemically.[17][16] |
Material entries describe families or representative grades, not an interchangeable specification for every spool. Test methods, orientations and conditions may differ. Unknown values are marked “Not documented”. Prices and source dates remain historical snapshots; check the linked guide for product details. Differences highlight text, not a universal winner.
Sources for this comparison
- eSUN PEBA-90A Technical Data Sheet v1.0 (Aug 2025), checked 2026-10-17 eSUN · 2025-08 · tds
- ThermaX PEEK Technical Data Sheet v3 3DXTech · 2026-08 · tds
- VICTREX AM 450 FIL — datasheet Victrex · 2025-12 · tds
- 3DXTech product catalogue 3DXTech · 2026-08 · vendor
- 3D4Makers product catalogue 3D4Makers · 2026-08 · vendor
- IEMAI 3D PEEK 3D Printing Filament — store page IEMAI 3D · 2026-08 · vendor
- eSUN PEBA-90A official product page: 1 kg price and product identity eSUN · 2026-10-17 · vendor
- Prusament PEI 1010 Technical Datasheet v1.0 Prusa Polymers · 2024-09 · tds
- Prusament PEI 1010 — material page Prusa Polymers · 2026-08 · doc
- ThermaX PEEK — product page 3DXTech · 2026-08 · vendor
- VICTREX AM 200 — FDM Material Data Sheet Stratasys · 2024-04 · tds
- TECAPEEK natural (PEEK) — stock shape properties Ensinger · 2026-08 · tds
- PEEK polymers — product overview Victrex · 2026-08 · doc
- Emissions of Ultrafine Particles and Volatile Organic Compounds from Commercially Available Desktop Three-Dimensional Printers with Multiple Filaments (Azimi et al.) Environmental Science & Technology 50(3) 1260-1268 · 2016-01 · paper
- The Effects of Sulfonated Poly(ether ether ketone) Ion Exchange Preparation Conditions on Membrane Properties Yee, Zhang & Ladewig, Membranes 3(3) 182–195 · 2013-07 · paper
- Chemical resistance — resistance of Ensinger plastics to chemicals (DIN 50 014, 23/50) Ensinger · 2026-08 · tds
- What solvents are not compatible with PEEK? — fluidics technical FAQ IDEX Health & Science · 2026-08 · doc