Filament comparison
PCTG vs HT soluble
Compare printing settings, strength, heat resistance, dated prices and sources.
2 selected · all documented properties
| Property | PCTGPETG | High-temperature supportSUPPORT |
|---|---|---|
| Market snapshot | ||
| Listing priceUSD/kg; dated snapshots | $34.99/kg median; $14.00–$50.67/kg across 5 dated product listings | $209.00/kg median; $100.00–$290.00/kg across 4 dated product listings |
| Identity & Market | ||
| Base polymer / chemistry | Poly(cyclohexylenedimethylene terephthalate) glycol — a copolyester with a higher cyclohexanedimethanol content than PETG[1][2] | Break-away support compounded to survive high-temperature print chambers; 3DXTech sells separate grades for PC/ABS and for the PAEK and PEI class[3][4] |
| Densityg/cm³ | 1.23 (Extrudr, ASTM D792; 3DXTech, ISO 1183)[2][5] | 1.37 (3DXTech THERMAX HTS1, ISO 1183)[3] |
| Typical priceUSD/kg | 1 kg spools cluster near 34[6][5][7] | 1 kg-equivalent spools cluster near 168[8] |
| Price range across brandsUSD/kg | 14–51 across brands; CHCKX 14 in a 10-roll bundle, Push Plastic 30, Proto-pasta 35 at 1 kg, 3DXTech 51[6][5][9] | 100–290 across grades; 3DXTech THERMAX MTS1 100 at 2 kg, HTS2 168 at 250 g, HTS1 250 at 500 g, IEMAI 3D HT-SP 290 at 1 kg[8][10] |
| Market availability1–5 | Available from several mainstream brands[6][5][7][11] | Niche, a handful of specialist brands[8][10] |
| Spool sizes & diameters | 1.75 and 2.85 mm; 0.5, 0.75, 1, 3 and 5 kg spools[6][7][5] | 1.75 mm; 250 g, 500 g, 1 kg and 2 kg spools[8] |
| Typical applications | Transparent covers, guards and impact-loaded parts where PETG cracks[1][2] | Support for PEEK, PEI and PC-class prints, where PVA and PLA-based supports would decompose[3][4] |
| Printing Parameters | ||
| Nozzle temperature°C | 250–270 (Spectrum, Extrudr)[1][2] | Not documented |
| Bed temperature°C | 60–100 (Spectrum)[1] | Not documented |
| Enclosure / chamber requirement1–5 | Open frame is fine — Spectrum and Extrudr both say a closed chamber is not necessary, Extrudr adds it helps on larger parts[1][2] | Actively heated chamber required — it is used inside high-temperature builds[3] |
| Part cooling fan | Up to 100 % (Spectrum); 20–50 % (Extrudr)[1][2] | Not documented |
| Bed surface & adhesion aid | Textured PEI, satin or powder-coated sheets; on smooth PEI a glue stick acts as a release agent[12][13] | Not documented |
| Maximum volumetric flow (mm³/s; see test conditions)mm³/s | 1.6–16 at the 20–200 mm/s Extrudr rates the material for, on a 0.4 mm nozzle at 0.2 mm layer[2][14] | Not documented |
| Bed-adhesion difficulty1–5 | Needs the right surface or a thin adhesive — the problem is releasing the part, not sticking it[12][13] | Not documented |
| Stringing / oozing tendency1–5 | Moderate — retraction tuning needed; Polymaker names stringing as PETG's common quirk[13] | Not documented |
| Shrinkage% | 0.2–0.5 (Extrudr, ASTM D955)[2] | Not documented |
| Overall printing difficulty1–5 | Easy — minor profile tuning[1][2] | Expert / industrial hardware only[3] |
| Extruder requirement | Not documented | A dual-extruder machine rated for high-temperature materials; 3DXTech states the grade is intended for dual-extruder printers designed to print high-temp materials[15] |
| Hardware Wear & Reliability | ||
| Nozzle hardness required1–4 | Brass fine indefinitely — Extrudr explicitly states no hardened nozzle is needed[2] | Brass fine indefinitely[3] |
| Abrasiveness1–5 | Non-abrasive[2] | Non-abrasive[3] |
| Nozzle clog risk1–5 | Low — 3DXTech lists no special nozzle concerns and no minimum layer height for PCTG, only a 65 °C pre-dry[16] | Moderate — needs dry filament and a clean nozzle; 3DXTech lists no special nozzle concerns but a mandatory 120 °C pre-dry for HTS1 and 80 °C for MTS1[15][17] |
| Heat-creep / jam sensitivity1–5 | Slightly sensitive[18] | Not documented |
| Hotend requirement | No special hot-end required[18] | Not documented |
| Moisture Behaviour | ||
| Moisture absorption (hygroscopicity)1–5 | Moderate (0.3–0.8 %) — the copolyester matrix reaches 0.40 % saturated at 25 °C / 55 % RH and 3DXTech specifies a 65 °C, 4 h pre-dry[12][16] | Not documented |
| Symptoms when wet | Bubbling and popping at the nozzle, stringing and a rough surface[19] | Not documented |
| Effect of moisture on strength | Polymaker groups PETG with nylon, PVA and TPU as highly hygroscopic; no dry-versus-conditioned strength figures are published for this grade and the loss shows as bubbling and poor layer adhesion[19] | No dry-versus-conditioned figures are published; 3DXTech mandates a 120 °C, 4 h pre-dry for HTS1 and 80 °C for MTS1 because trapped water flashes to steam at these nozzle temperatures[15][17] |
| Storage requirement | Sealed with desiccant; Polymaker groups PETG with the highly hygroscopic materials[19][13] | Not documented |
| Mechanical Properties | ||
| Tensile strength (XY)MPa | 43–44 at yield and 45–46 at break (ISO 527, injection-moulded resin data from Spectrum and Extrudr); 48 on My Tech Fun printed bars[1][2][20] | Not documented |
| Elongation at break% | 215–220 at break on moulded specimens (ISO 527); 4.3–4.4 at yield[1][2] | Not documented |
| Charpy impact, notchedkJ/m² | 93–94 notched Izod at 23 °C on moulded specimens (ISO 180); 3DXTech quotes 8 by ISO 180/A[1][2][5] | Not documented |
| Other impact data | Izod 4.14 kJ/m² on My Tech Fun printed bars, against 3.37 for PETG on the same rig[20] | Not documented |
| Layer adhesion / Z tensileMPa | 21.6 on My Tech Fun 4×4 mm printed bars, against 32.9 for PETG[20] | Not documented |
| Brittleness1–5 | Tough — absorbs impact, yields before breaking[1][2] | Not documented |
| Hardness (scale-specific)Shore A / Shore D / Rockwell | 69 Shore D measured by My Tech Fun, against 72 for PETG[20] | Not documented |
| Creep resistance / sustained load1–5 | Below average — a 12 mm bar sagged to 19.4 mm over 5 days at 1.25 kg, slightly worse than PETG's 18.2[20] | Not documented |
| Fatigue / repeated-flex resistance1–5 | Good — 215 % elongation at break and 94 kJ/m² notched Izod on moulded specimens (Extrudr, Spectrum)[1][2] | Not documented |
| Elasticity / flexibility1–5 | Slightly flexible in thin sections[20] | Not documented |
| Wear resistance & friction | Not documented | 3DXTech marks tensile strength, modulus and elongation as not applicable for its support grades — they are not characterised as structural materials[3] |
| Thermal Properties | ||
| HDT at 1.8 MPa°C | Not documented | 205 (THERMAX HTS1, printed XY, ISO 75 at 1.8 MPa)[3] |
| Glass transition (Tg)°C | 78 (3DXTech, DSC)[5] | 225 (3DXTech THERMAX HTS1, DSC) — high enough to stay solid inside a PEI or PEEK build[3] |
| Melting point / Vicat°C | Amorphous — no melting point; Vicat 88 (Spectrum, Extrudr)[1][2] | Not documented |
| Continuous service temperature°C | 68 — loaded bars begin to move at this temperature, against 65 for PETG[20] | Not documented |
| Flammability / UL 94 | Flammable; no UL 94 rating published for standard grades[21] | Not documented |
| Environment & Chemical | ||
| Chemical resistance | Withstands acids, alkalis, oils and UV exposure[13] | Not documented |
| Water / humidity resistance in service1–5 | Good — minor absorption; Spectrum describes the polymer as hydrophobic[1] | Not documented |
| Food contact | Not certified for food contact as filament[13] | Not documented |
| Biodegradability / compostability | Not biodegradable[13] | Not documented |
| Recyclability | Not accepted in household plastic collection[13] | Not documented |
| Electrical & ESD properties | Surface resistance above 10¹³ ohm/sq — insulating (3DXTech, ASTM D257)[5] | Surface resistance above 10^13 ohm/sq on all three THERMAX support grades (ASTM D257) — insulating[3][22][4] |
| Health & Safety | ||
| Fume toxicity1–5 | Moderate — measurable VOCs and UFPs, ventilation advised[23] | Low hazard — minimal VOC and particle emission; none of these materials was in the chamber study[23] |
| Ventilation / filtration requirement1–5 | Open a window / occasional ventilation[23] | Open a window / occasional ventilation[23] |
| Post-Processing | ||
| Sanding & machining | Sands poorly — the material is tough and gums rather than powders[18] | Not documented |
| Gluing & solvent welding | Cyanoacrylate; no common solvent welds PETG cleanly[18] | Not documented |
| Vapour / chemical smoothing | No practical vapour smoothing[18] | Not documented |
| Support material pairing | Prints its own supports; Polymaker rates PolyDissolve S1 for PETG[18] | This is the support material. MTS1 is matched to PC/ABS and PC; HTS1 and HTS2 to the higher-temperature classes[4][3] |
| Dimensional accuracy & detail | Optical clarity is the selling point; Extrudr recommends a layer height at most 50 % of nozzle diameter[2] | Not documented |
| Solvents & Solubility | ||
| Soluble in | No common workshop solvent; Eastman's CHDM copolyester data shows 1,2-dichloroethane destroying it within a week.[24] | Aqueous alkali, not water: IEMAI specifies an alkaline bath in an ultrasonic cleaner until the support dissolves.[10] |
| Softened or crazed by | Acetone, ethyl acetate, toluene and DMF swell and soften the copolyester; methanol crazes it (Eastman, 1 y at 23 °C).[24] | Not documented |
| Solvent welding & smoothing agent | Dichloromethane brushed on is the only agent that smooths PETG — a controlled carcinogen, not workshop stock.[25] | None — the alkaline bath dissolves the support rather than welding anything.[10] |
Material entries describe families or representative grades, not an interchangeable specification for every spool. Test methods, orientations and conditions may differ. Unknown values are marked “Not documented”. Prices and source dates remain historical snapshots; check the linked guide for product details. Differences highlight text, not a universal winner.
Sources for this comparison
- Spectrum Premium PCTG Technical Data Sheet Spectrum Filaments · 2026-08 · tds
- Extrudr PCTG technical data Extrudr · 2026-08 · tds
- THERMAX HTS1 Break Away Support Technical Data Sheet v1.0 3DXTech · 2026-08 · tds
- THERMAX MTS1 Break Away Support Technical Data Sheet v1.0 3DXTech · 2026-08 · tds
- MAX-G PCTG Technical Data Sheet 3DXTech · 2026-08 · tds
- Push Plastic product catalogue Push Plastic · 2026-08 · vendor
- Proto-pasta product catalogue Proto-pasta · 2026-08 · vendor
- 3DXTech product catalogue 3DXTech · 2026-08 · vendor
- CHCKX 10KG Multicolor PCTG Filament bundle CHCKX (Amazon US) · 2026-08 · vendor
- IEMAI 3D HT-SP alkaline-soluble support filament — store page IEMAI 3D · 2026-08 · vendor
- Atomic Filament product catalogue Atomic Filament · 2026-08 · vendor
- Prusament PETG Technical Datasheet v1.1 Prusa Polymers · 2022-02 · tds
- PETG — material basics Polymaker Wiki · 2026-08 · doc
- Max volumetric speed Prusa Knowledge Base · 2026-08 · doc
- THERMAX HTS1 — product page 3DXTech · 2026-08 · vendor
- MAX-G PCTG — product page (print recommendations) 3DXTech · 2026-08 · doc
- THERMAX MTS1 — product page 3DXTech · 2026-08 · vendor
- PET and PETG — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- Wet Filament — signs, causes and drying Polymaker Wiki · 2026-08 · doc
- PCTG vs PETG comparison — results spreadsheet My Tech Fun (Igor Gaspar) · 2026-08 · test
- Prusament PETG V0 Technical Datasheet Prusa Polymers · 2026-08 · tds
- THERMAX HTS2 Break Away Support Technical Data Sheet v1.0 3DXTech · 2026-08 · tds
- Emissions of Ultrafine Particles and Volatile Organic Compounds from Commercially Available Desktop Three-Dimensional Printers with Multiple Filaments (Azimi et al.) Environmental Science & Technology 50(3) 1260-1268 · 2016-01 · paper
- Eastman Spectar copolyester — Chemical resistance (unstressed bars, 1 year at 23 °C) Eastman Chemical Company · 2026-08 · tds
- Improve your 3D prints with chemical smoothing Prusa Research · 2026-08 · doc