Filament comparison
ASA-CF vs PA12-GF
Compare printing settings, strength, heat resistance, dated prices and sources.
2 selected · all documented properties
| Property | Carbon-fibre ASA (ASA-CF)ASA | Glass-fibre PA12 (PA12-GF)PA |
|---|---|---|
| Market snapshot | ||
| Listing priceUSD/kg; dated snapshots | $36.99/kg median; $25.00–$90.00/kg across 5 dated product listings | $130.67/kg median; $46.00–$140.18/kg across 3 dated product listings |
| Identity & Market | ||
| Base polymer / chemistry | ASA reinforced with chopped carbon fibre — Formfutura's ApolloX CF10 is 10 wt%[1][2][3] | PA12 reinforced with chopped glass fibre — 3DXTech's grade is nominally 30 wt%[4] |
| Densityg/cm³ | 1.02 (Bambu Lab), 1.1 (Formfutura ApolloX CF10) and 1.11 (3DXTech), ISO 1183[1][2][3] | 1.23 (ISO 1183)[4] |
| Typical priceUSD/kg | 1 kg spools cluster near 37[5][6] | 1 kg-equivalent spools span 46–140; the middle of the market is about 88[7][8][9] |
| Price range across brandsUSD/kg | 25–90 across brands; IEMAI 25, Ambrosia 33, Bambu Lab 37, Polymaker Fiberon 40, 3DXTech 90[10][5][6][7][11] | 46–140 across brands; IEMAI 3D 46, 3DXTech 131 at 750 g and 130 at 2 kg, PrimaCreator NylonPower Glass Fiber 140 at 500 g[7][8][9] |
| Market availability1–5 | Available from several mainstream brands[5][6][7][10] | Available from several mainstream brands[7][8] |
| Spool sizes & diameters | 1.75 and 2.85 mm; 0.5, 0.75 and 1 kg spools[6][7][5] | 1.75 and 2.85 mm; 0.5, 0.75 and 2 kg spools[7][9] |
| Typical applications | Outdoor structural parts, drone and antenna mounts where stiffness and UV stability both matter[1][2] | Stiff, humidity-stable structural parts — the glass gives the modulus, the PA12 matrix limits the moisture drift[4][12] |
| Printing Parameters | ||
| Nozzle temperature°C | 250–280 (Bambu Lab)[1] | Not documented |
| Bed temperature°C | 80–100 (Bambu Lab)[1] | Not documented |
| Enclosure / chamber requirement1–5 | Enclosure recommended — Bambu Lab specifies a 45–60 °C chamber[1][13] | Enclosure required (passive)[14] |
| Recommended chamber temperature°C | 45–60 (Bambu Lab)[1] | Not documented |
| Part cooling fan | Fan on (Bambu Lab)[1] | Not documented |
| Bed surface & adhesion aid | PEI sheet, BuildTak or an adhesion aid such as Magigoo (Polymaker); Simplify3D also lists Kapton tape and ASA slurry[15][16] | PEI sheet with a glue stick, or a dedicated adhesive such as Magigoo[17][14] |
| Maximum volumetric flow (mm³/s; see test conditions)mm³/s | 20 at Bambu Lab's 250 mm/s cap on a 0.4 mm nozzle at 0.2 mm layer[1][18] | Not documented |
| Warping tendency1–5 | Moderate — needs adhesion aid or draught shield; the fibre reduces warping against unfilled ASA[13] | Not documented |
| Bed-adhesion difficulty1–5 | Needs a specific surface plus adhesive[15] | Needs a specific surface plus adhesive[17] |
| Stringing / oozing tendency1–5 | Slight — Polymaker advises 1–2 mm retraction at 20–30 mm/s[15] | Moderate — retraction tuning needed[14] |
| Overall printing difficulty1–5 | Intermediate — dry filament and a tuned profile; hardened nozzle mandatory[13] | Advanced — enclosure, hardware upgrades, tuning[14] |
| Hardware Wear & Reliability | ||
| Nozzle hardness required1–4 | Hardened steel required[13] | Hardened steel required — no nozzle-life figure is published for a PA12-GF30 grade; Polymaker measures about 9 h of brass nozzle life on its comparable fibre-filled nylons[19] |
| Abrasiveness1–5 | Highly abrasive — standard CF composite[13] | Highly abrasive — standard GF composite[19] |
| Nozzle clog risk1–5 | Moderate — needs dry filament and a clean nozzle; Prusa lists higher risk of nozzle clogging for fibre-filled composites and Simplify3D a higher tendency to clog[20][21] | High — jams from moisture, heat creep or particles[22] |
| Heat-creep / jam sensitivity1–5 | Slightly sensitive[16] | Moderate — good heatbreak cooling needed[17] |
| Hotend requirement | No special hotend required[16] | May require an all-metal hot end (Simplify3D)[17] |
| Moisture Behaviour | ||
| Moisture absorption (hygroscopicity)1–5 | Moderate — 0.33 % saturated at 25 °C / 55 % RH (Bambu Lab)[1] | High (0.8–2 %) — the PA12 matrix takes up far less than PA6, on the evidence of Polymaker's 1.5 % for PA12-CF10 against 3.33 % for PA6-GF25[23][24] |
| Equilibrium moisture content at ~50 % RH% | 0.33 saturated at 25 °C / 55 % RH (Bambu Lab)[1] | Not documented |
| Drying temperature & time | 80 °C for 8 h (Bambu Lab)[1] | Not documented |
| Symptoms when wet | Bubbling and popping at the nozzle, stringing and a rough surface[22] | Not documented |
| Effect of moisture on strength | No dry-versus-conditioned figures are published; Polymaker groups the styrenics as moderate-sensitivity and absorbed water shows as bubbling and poor layer adhesion[22] | Polymaker's PA12 grades change little between wet and dry, unlike PA6; the CoPA dry-to-wet blocks show the PA6-type response[12][25] |
| Storage requirement | Sealed with desiccant; Polymaker rates the styrenics moderate-sensitivity[22] | Sealed below 20 % RH with desiccant[22] |
| Hydrolysis at melt temperature | Not documented | Polymaker specifies an 80–100 °C dry and storage below 20 % RH; no molecular-weight loss figure is published, and the wet data it does publish is conditioning rather than melt hydrolysis[19][25] |
| Mechanical Properties | ||
| Tensile strength (XY)MPa | 34 ± 3 printed XY, ISO 527 (Bambu Lab); 3DXTech quotes 48 at break and Formfutura 79 at 23 °C[1][2][3] | 82 at break (printed XY, ISO 527)[4] |
| Young's modulusMPa | 4200 ± 270 printed XY, ISO 527 (Bambu Lab); 3DXTech quotes 5355 and Formfutura 7580[1][2][3] | 7800 (printed XY, ISO 527)[4] |
| Elongation at break% | 9.6 ± 1.4 printed XY, ISO 527 (Bambu Lab); 3DXTech quotes 3 at break and Formfutura 1.8[1][2][3] | 4.5 at break (printed XY, ISO 527) — nearly double the 2.4 % of Polymaker's PA6-GF25[4][24] |
| Flexural strengthMPa | 72 ± 5 printed XY, ISO 178 (Bambu Lab); 3DXTech quotes 78[1][2] | 94 (printed XY, ISO 178)[4] |
| Flexural modulusMPa | 3740 ± 130 printed XY, ISO 178 (Bambu Lab); 3DXTech quotes 5210[1][2] | 7550 (printed XY, ISO 178)[4] |
| Charpy impact, notchedkJ/m² | 6.2 ± 1.4 printed XY, ISO 179, notched (Bambu Lab) — a third of unfilled Bambu Lab ASA's 19.6[1][26] | Not documented |
| Other impact data | Charpy unnotched 14.0 ± 2.2 printed XY (Bambu Lab, ISO 179), against 41.0 for unfilled Bambu Lab ASA[1][26] | Not documented |
| Layer adhesion / Z tensileMPa | 30 ± 4 printed Z, ISO 527 (Bambu Lab); flexural Z falls to 33 against 72 in XY[1] | Not documented |
| Brittleness1–5 | Brittle — snaps with little warning[1][2] | Moderate[4] |
| Hardness (scale-specific)Shore A / Shore D / Rockwell | Not documented | Rockwell M88 / R117 on extruded PA66-GF30 stock (ASTM D785); no figure is published for a glass-fibre PA12 filament[27] |
| Creep resistance / sustained load1–5 | Good — no creep test found; chopped carbon fibre lifts modulus to 4200 MPa against 2379–2450 for unfilled ASA[1][28] | Good. Ensinger lists high creep resistance for extruded PA66-GF30 stock, and the PA12 matrix absorbs far less water than PA6, so a PA12-GF part holds load better in a humid environment[27][14] |
| Fatigue / repeated-flex resistance1–5 | Below average — no CF-grade S-N curve; notched Charpy falls to 6.2 kJ/m² against 19.6 for unfilled Bambu Lab ASA[1][26] | Good. Ensinger lists high fatigue strength as a headline property of extruded PA66-GF30 stock[27] |
| Elasticity / flexibility1–5 | Rigid[1] | Rigid[4] |
| Z strength as % of XY% | 88 by tensile, 46 by flexural (printed, Bambu Lab)[1] | Not documented |
| Thermal Properties | ||
| HDT at 0.45 MPa°C | 110 (ISO 75, 0.45 MPa, Bambu Lab) against 100 for unfilled Bambu Lab ASA[1][26] | Not documented |
| HDT at 1.8 MPa°C | 102 (ISO 75, 1.8 MPa, Bambu Lab) against 92 for unfilled Bambu Lab ASA[1][26] | Not documented |
| Continuous service temperature°C | 93 — Prusa publishes this as the temperature resistance of Prusament ASA[29] | Not documented |
| Thermal expansion (CTE)µm/m·K | Not documented | 48.6 on extruded PA66-GF30 stock (ASTM D696; source states 2.7e-5 in/in/°F) — no figure is published for a glass-fibre PA12 filament[27] |
| Flammability / UL 94 | Flammable; no UL 94 rating published[26] | Flammable; no UL 94 rating published for the grades surveyed[19] |
| Environment & Chemical | ||
| UV resistance1–5 | Excellent — designed for permanent outdoor use; the acrylate rubber phase is unchanged by the fibre[30][15] | Months outdoors before embrittlement — unstabilised polyamide yellows under UV[14] |
| Chemical resistance | Good against weak acids, weak alkalis, oils and grease; dissolved by acetone[28] | Withstands oils, fuels and alkalis[14] |
| Water / humidity resistance in service1–5 | Not documented | Good — minor absorption relative to PA6-based composites[12] |
| Food contact | Not food safe[15] | Not food-contact certified as filament[14] |
| Biodegradability / compostability | Not biodegradable[15] | Not biodegradable[14] |
| Recyclability | Not accepted in household plastic collection[15] | Not accepted in household plastic collection[14] |
| Electrical & ESD properties | Surface resistance above 10⁹ ohm/sq — not static-dissipative (3DXTech, ASTM D257)[2] | Surface resistance above 10¹³ ohm/sq — insulating (ASTM D257)[4] |
| Health & Safety | ||
| Fume toxicity1–5 | High — hazardous VOC such as styrene; enclosure and filtration needed[31][13] | Moderate — measurable VOCs and UFPs, ventilation advised[31] |
| VOC emission rateµg/min | Not documented | Up to 180 caprolactam, the dominant VOC from nylon and the largest single-VOC rate in the study[31] |
| Ultrafine-particle emission rateparticles/min | Not documented | ≈2 × 10⁸ median for nylon — low for particles despite the highest VOC mass measured[31] |
| Hazardous species emitted | Styrene. Bambu Lab states ABS and ASA release harmful gases such as styrene at printing temperature, which can be toxic and cause dizziness or nausea. Azimi et al. measured styrene from every styrenic filament tested but did not test ASA itself[13][31] | Caprolactam, at up to 180 µg/min from nylon filament[31] |
| Ventilation / filtration requirement1–5 | Enclosure with carbon and HEPA filtration[31][13] | Ventilated room or enclosure recommended[31] |
| Dust & fibre handling hazard | Carbon fibre is bound in the matrix; sanding dust should not be inhaled[2] | Glass fibre is bound in the matrix; avoid inhaling sanding dust[4] |
| Post-Processing | ||
| Sanding & machining | Sands well and takes filler before painting[15] | Sands poorly — gums rather than powders[17] |
| Painting & finishing | Paints readily; ASA holds colour outdoors so many parts are left unpainted[15] | Not documented |
| Gluing & solvent welding | Solvent-welds with acetone[28] | Cyanoacrylate; no common solvent welds polyamide[17] |
| Vapour / chemical smoothing | Acetone vapour smoothing works[28] | No practical vapour smoothing[17] |
| Support material pairing | HIPS breaks away or dissolves in d-limonene; Bambu Lab sells a Support for ABS that also serves ASA[13] | Not documented |
| Dimensional accuracy & detail | Matte fibre-filled finish hides layer lines[1] | Not documented |
| Solvents & Solubility | ||
| Soluble in | Acetone dissolves the resin and leaves the fibre; MEK, THF, ethyl acetate and chlorinated solvents attack the styrenic backbone.[32][28] | Formic acid, phenol, m-cresol and hexafluoroisopropanol dissolve the matrix at 23 °C, leaving the fibre; laboratory reagents.[33] |
| Softened or crazed by | Limonene attacks some grades — Prusa reports Prusament ASA Orange flaking apart as layer adhesion fails.[34] | Zinc chloride solutions stress-crack the nylon matrix, alcoholic calcium chloride dissolves it, mineral acids attack it.[33] |
| Solvent welding & smoothing agent | Acetone vapour reaches only the resin fraction, so the fibre is left standing proud of the smoothed surface.[35][28] | None — nylon's only solvents (formic acid, phenol, HFIP) degrade the part, and the fibre blocks surface flow anyway.[33] |
Material entries describe families or representative grades, not an interchangeable specification for every spool. Test methods, orientations and conditions may differ. Unknown values are marked “Not documented”. Prices and source dates remain historical snapshots; check the linked guide for product details. Differences highlight text, not a universal winner.
Sources for this comparison
- Bambu Filament Technical Data Sheet V1.0 — ASA-CF Bambu Lab · 2026-08 · tds
- CarbonX Carbon Fiber ASA Technical Data Sheet 3DXTech · 2026-08 · tds
- ApolloX CF10 Technical Data Sheet Formfutura · 2026-08 · tds
- FibreX PA12-GF30 Technical Data Sheet v1.0 3DXTech · 2026-08 · tds
- ASA-CF — product page Bambu Lab US Store · 2026-08 · vendor
- Polymaker product catalogue Polymaker · 2026-08 · vendor
- 3DXTech product catalogue 3DXTech · 2026-08 · vendor
- IEMAI 3D GF-PA12 3D Printing Filament — store page IEMAI 3D · 2026-08 · vendor
- PrimaCreator SELECT NylonPower Glass Fiber product page PrimaCreator · 2026-08 · vendor
- Filastruder product catalogue Filastruder · 2026-08 · vendor
- IEMAI CF-ASA 3D Printing Filament product page IEMAI 3D · 2026-08 · vendor
- Moisture Conditioning — effect on printed nylon properties Polymaker Wiki · 2026-08 · doc
- ABS / ASA / PC Usage Guide Bambu Lab Wiki · 2026-08 · doc
- PA (Nylon) — material basics Polymaker Wiki · 2026-08 · doc
- ASA — material basics Polymaker Wiki · 2026-08 · doc
- ASA — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- Nylon — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- Max volumetric speed Prusa Knowledge Base · 2026-08 · doc
- Fiberon PA6-CF20 Technical Data Sheet V1.1 Polymaker · 2024-12 · tds
- Composite materials filled with carbon, kevlar or glass Prusa Knowledge Base · 2026-08 · doc
- Carbon Fiber Filled — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- Wet Filament — signs, causes and drying Polymaker Wiki · 2026-08 · doc
- Fiberon PA12-CF10 Technical Data Sheet V1.1 Polymaker · 2025-02 · tds
- Fiberon PA6-GF25 Technical Data Sheet V1.1 Polymaker · 2024-12 · tds
- PolyMide CoPA Technical Data Sheet V5.4 (dry and wet status blocks) Polymaker · 2024-11 · tds
- Bambu Filament Technical Data Sheet V3.0 — ASA Bambu Lab · 2026-08 · tds
- TECAMID 66 GF30 black (PA66-GF30) — stock shape properties Ensinger · 2026-08 · tds
- PolyLite ASA Technical Data Sheet Polymaker · 2024-11 · tds
- Prusament ASA — material page Prusa Polymers · 2026-08 · doc
- ASA — FDM Material Data Sheet (includes 1000 h QUV exposure results) Stratasys · 2026-08 · tds
- Emissions of Ultrafine Particles and Volatile Organic Compounds from Commercially Available Desktop Three-Dimensional Printers with Multiple Filaments (Azimi et al.) Environmental Science & Technology 50(3) 1260-1268 · 2016-01 · paper
- Chemical resistance — resistance of Ensinger plastics to chemicals (DIN 50 014, 23/50) Ensinger · 2026-08 · tds
- Ultramid Nylon Chemical Resistance guide (unmodified PA6 B27E and PA66 A27E) BASF · 2026-08 · tds
- HIPS — Knowledge Base Prusa Research · 2026-08 · doc
- Improve your 3D prints with chemical smoothing Prusa Research · 2026-08 · doc