| Property | ABS+ / Tough ABSABS | Glass-fibre PC (PC-GF)PC |
|---|---|---|
| Market snapshot | ||
| Listing priceUSD/kg; dated snapshots | $26.49/kg median; $15.99–$29.99/kg across 4 dated product listings | $71.27/kg median; $71.27–$71.27/kg across 1 dated product listings |
| Identity & Market | ||
| Base polymer / chemistry | ABS reformulated for lower warping and a higher glass transition; Polymaker's ABS Pro and ABS Max reach Tg 114.9 and 126.3 °C against 101 °C for PolyLite ABS[1][2][3] | Polycarbonate reinforced with 30 wt% short glass fibre[4] |
| Densityg/cm³ | 1.04 (ABS Pro) and 1.06 (ABS Max), ISO 1183[1][2] | 1.17 (measured on a 100 % infill printed part, ISO 1183-A)[4] |
| Typical priceUSD/kg | 1 kg spools cluster near 27[5] | 1 kg spools cluster near 71[6] |
| Price range across brandsUSD/kg | 16–30 across brands; SUNLU E-ABS 16, Polymaker ABS Pro 25, YXPOLYER ABS Enhanced 28, Polymaker ABS Max 30[5][7][8] | 71 — BASF Ultrafuse PC GF30 at igo3d is the only priced listing found; Owens Corning sells XSTRAND GF30-PC in 500 g and 1 kg[6][4] |
| Market availability1–5 | Available from several mainstream brands[5] | Niche, a handful of specialist brands — neither Polymaker's nor 3DXTech's polycarbonate range contains a glass-fibre grade, but BASF Forward AM and Owens Corning both sell one through European retail[6][4][5][9] |
| Spool sizes & diameters | 1.75 and 2.85 mm; 1 kg spools[5] | 1.75 and 2.85 mm at +/- 0.05 mm; 500 g and 1 kg net spools[4] |
| Typical applications | Large enclosure and automotive parts where plain ABS warps or softens too early[1][2] | Functional prototyping for mechanical engineering, electronics and automotive[4] |
| Diameter tolerance± mm | Not documented | +/- 0.05 (Owens Corning XSTRAND)[4] |
| Printing Parameters | ||
| Nozzle temperature°C | 270–290 (ABS Pro); 270–300 (ABS Max) — 25–35 °C above plain ABS[1][2] | 280-330 (Owens Corning XSTRAND GF30-PC)[4] |
| Bed temperature°C | 120 (ABS Max)[2] | 80-110 (Owens Corning XSTRAND GF30-PC)[4] |
| Enclosure / chamber requirement1–5 | Enclosure required (passive)[1][2][10] | Enclosure required (passive) — as for unfilled PC[11][10] |
| Bed surface & adhesion aid | Clean the plate and apply glue; Simplify3D also lists Kapton tape and ABS slurry[10][12] | Perforated plate, DimaFix or Magigoo PC glue (Owens Corning)[4] |
| Maximum volumetric flow (mm³/s; see test conditions)mm³/s | Up to 250 mm/s (ABS Pro) and 200 mm/s (ABS Max), equivalent to 20 and 16 on a 0.4 mm nozzle at 0.2 mm layer[1][2][13] | Not documented |
| Warping tendency1–5 | High — enclosure needed for reliable large parts[10] | Not documented |
| Bed-adhesion difficulty1–5 | Needs a specific surface plus adhesive[10] | Not documented |
| Stringing / oozing tendency1–5 | Slight — Polymaker advises 1–2 mm retraction at 20–30 mm/s[14] | Not documented |
| Overall printing difficulty1–5 | Intermediate — dry filament and a tuned profile; the hotter nozzle rules out PTFE-lined hotends[1][2] | Not documented |
| Extruder requirement | Not documented | Owens Corning specifies a nozzle above 0.4 mm and hardened steel nozzles and drive wheels[4] |
| Hardware Wear & Reliability | ||
| Nozzle hardness required1–4 | Brass fine indefinitely[10] | Hardened steel required — Owens Corning states glass reinforcement shortens brass nozzle and drive-wheel life[4] |
| Abrasiveness1–5 | Non-abrasive[10] | Highly abrasive — 30 wt% glass fibre[4] |
| Nozzle clog risk1–5 | Low — unfilled ABS compound; no special hot-end required and clogging is not among the listed drawbacks[12][15] | High — jams from moisture, heat creep or particles; PC already absorbs water from the air and Prusa lists glass-filled composites as a higher clogging risk[16][17] |
| Heat-creep / jam sensitivity1–5 | Slightly sensitive[12] | Not documented |
| Hotend requirement | No special hot-end required[12] | Not documented |
| Moisture Behaviour | ||
| Moisture absorption (hygroscopicity)1–5 | Moderate — 0.51 % maximum water absorption (ABS Pro)[1] | Negligible (<0.1 % EMC) — Owens Corning measures below 0.1 % at 23 °C and 50 % RH (ISO 62)[4] |
| Equilibrium moisture content at ~50 % RH% | 0.51 maximum water absorption (Polymaker ABS Pro)[1] | Below 0.1 at 23 °C and 50 % RH, and below 0.1 at saturation (ISO 62)[4] |
| Drying temperature & time | 70 °C for 6 h (ABS Max)[2] | Not documented |
| Symptoms when wet | Bubbling and popping at the nozzle, stringing and a rough surface[18] | Not documented |
| Effect of moisture on strength | Polymaker rates ABS moderate-sensitivity and publishes no dry-versus-conditioned figures[18] | No dry-versus-conditioned figures are published. Polymaker calls PC highly hygroscopic; absorbed water flashes to steam and shows as bubbling and poor layer adhesion[19][18] |
| Storage requirement | Sealed with desiccant; Polymaker rates ABS moderate-sensitivity[18] | Not documented |
| Mechanical Properties | ||
| Tensile strength (XY)MPa | 34.9 (ABS Pro) and 35.7 (ABS Max) printed XY, ISO 527[1][2] | 65 at break (printed, ISO 527 at 1 mm/min)[4] |
| Young's modulusMPa | 2330 (ABS Pro) and 2320 (ABS Max) printed XY, ISO 527[1][2] | 5400 (printed, ISO 527 at 1 mm/min)[4] |
| Elongation at break% | 6.7 (ABS Max) and 7.3 (ABS Pro) at break, printed XY, ISO 527[1][2] | 2.5 at break (printed, ISO 527 at 1 mm/min)[4] |
| Flexural strengthMPa | 60.1 (ABS Pro) and 63.3 (ABS Max) printed XY, ISO 178[1][2] | 113 at yield (printed, ISO 178 at 2 mm/min)[4] |
| Flexural modulusMPa | 2330 (ABS Pro) and 2500 (ABS Max) printed XY, ISO 178[1][2] | 5500 (printed, ISO 178 at 2 mm/min)[4] |
| Charpy impact, notchedkJ/m² | 10.5 (ABS Max) and 14.5 (ABS Pro) printed XY, ISO 179, notched[1][2] | Not documented |
| Layer adhesion / Z tensileMPa | 21.9 (ABS Pro) and 25.4 (ABS Max) printed Z, ISO 527[1][2] | Not documented |
| Brittleness1–5 | Tough — absorbs impact, yields before breaking[1][2] | Brittle — snaps with little warning; 2.5 % elongation at break[4] |
| Hardness (scale-specific)Shore A / Shore D / Rockwell | Not documented | Rockwell 70 (118) — the source does not name the scales and Shore D 79 on extruded unfilled PC stock (ASTM D785, D2240); no figure is published for a glass-fibre grade[20] |
| Creep resistance / sustained load1–5 | Moderate — no creep test found; Tg of 115 °C (ABS Pro) and 126 °C (ABS Max) keeps room-temperature service far below softening[1][2] | Excellent — holds load for years. Room-temperature tensile creep of moulded unfilled PC ran unbroken at 41 MPa until the test was stopped, and 30 wt% glass raises the tensile modulus from about 2.3 to 5.4 GPa[21][4] |
| Fatigue / repeated-flex resistance1–5 | Moderate — no S-N curve found; 6.7–7.3 % elongation and 10.5–14.5 kJ/m² notched Charpy, below unfilled Bambu Lab ABS[1][2][22] | Not documented |
| Elasticity / flexibility1–5 | Rigid[1] | Rigid[4] |
| Z strength as % of XY% | 63 (ABS Pro) and 71 (ABS Max), printed[1][2] | Not documented |
| Thermal Properties | ||
| HDT at 0.45 MPa°C | 106.4 (ABS Pro) and 118.1 (ABS Max), ISO 75 at 0.45 MPa[1][2] | Not documented |
| HDT at 1.8 MPa°C | 101.4 (ABS Pro) and 113.1 (ABS Max), ISO 75 at 1.8 MPa[1][2] | 137 (printed, ISO 75 Method A at 1.8 MPa)[4] |
| Glass transition (Tg)°C | 114.9 (ABS Pro) and 126.3 (ABS Max), DSC[1][2] | 145 (DSC, ISO 11357)[4] |
| Melting point / Vicat°C | Amorphous — no melting point; Vicat 116.1 (ABS Pro) and 127.4 (ABS Max), ISO 306[1][2] | 270 stated as melting point (ISO 11357) — unusual for an amorphous polymer, but this is the published figure[4] |
| Thermal expansion (CTE)µm/m·K | 86–89 for printed unfilled ABS (fibre Bragg grating, 25–50 °C); no grade-specific measurement published[23] | 26.2 in XY and 77.4 in Z (printed, ISO 11359-2) — a threefold anisotropy, and the lowest in-plane expansion of any polycarbonate here[4] |
| Flammability / UL 94 | Not documented | UL 94 V-0 verified (Owens Corning)[4] |
| Environment & Chemical | ||
| UV resistance1–5 | Months outdoors before embrittlement[14] | Good — years with some colour shift. Owens Corning lists UV resistance as a product benefit but publishes no exposure data[4] |
| Chemical resistance | Good against weak acids, weak alkalis, oils and grease; dissolved by acetone[3] | Not documented |
| Water / humidity resistance in service1–5 | Not documented | Excellent — essentially unaffected; below 0.1 % water at saturation (ISO 62)[4] |
| Food contact | Not food safe — Polymaker cites potential chemical leaching[14] | Not documented |
| Biodegradability / compostability | Not biodegradable[14] | Not documented |
| Recyclability | Mechanically recyclable but not accepted in household plastic collection[14] | Not documented |
| Electrical & ESD properties | Not documented | Electrically insulating (Owens Corning)[4] |
| Health & Safety | ||
| Fume toxicity1–5 | High — hazardous VOC such as styrene; enclosure and filtration needed[24][10] | Moderate — measurable VOCs and UFPs, ventilation advised[24] |
| VOC emission rateµg/min | 12–113 styrene, the dominant VOC from every ABS and HIPS combination tested[24] | Not documented |
| Ultrafine-particle emission rateparticles/min | 2 × 10¹⁰ to 9 × 10¹⁰ median across all ABS printers, two orders of magnitude above PLA's ≈1 × 10⁸[24] | ≈4 × 10¹⁰ median — the highest ultrafine-particle rate of the nine filaments in the chamber study, above every ABS tested[24] |
| Hazardous species emitted | Styrene dominates. Bambu Lab states ABS and ASA release harmful gases such as styrene at printing temperature, which can be toxic and cause dizziness or nausea[24][10] | Not documented |
| Ventilation / filtration requirement1–5 | Enclosure with carbon and HEPA filtration — an enclosure alone cut measured UFP by only about 35 %[24][10] | Ventilated room or enclosure recommended[24][10] |
| Dust & fibre handling hazard | Not documented | Owens Corning warns that the glass reinforcement is abrasive when melted and advises sufficient ventilation and avoiding extrusion fumes[4] |
| Post-Processing | ||
| Sanding & machining | Sands well and takes filler before painting[14] | Not documented |
| Painting & finishing | Paints readily after light abrasion[14] | Not documented |
| Vapour / chemical smoothing | Acetone vapour smoothing works[3] | Not documented |
| Support material pairing | HIPS breaks away or dissolves in d-limonene; Bambu Lab sells a dedicated Support for ABS[25][10] | Not documented |
| Dimensional accuracy & detail | Not documented | High dimensional stability is the headline benefit; the 26.2 um/m*K in-plane CTE is a third of unfilled PC's[4] |
| Solvents & Solubility | ||
| Soluble in | Acetone dissolves it — the basis of ABS slurry; so do MEK, THF, ethyl acetate, chloroform, dichloromethane and toluene.[26][3] | Dichloromethane and chloroform dissolve the matrix and leave the fibre; DMF and dioxane do the same (Covestro).[27] |
| Softened or crazed by | Petrol and perchloroethylene soften it and benzene attacks it; d-limonene disrupts layer adhesion in some ABS and ASA grades.[26][28] | Methanol, butyl acetate, ether, 1 % NaOH and phthalate plasticisers stress-crack it; acetone, MEK and xylene swell it.[27] |
| Solvent welding & smoothing agent | Acetone: about 20 min of vapour at 80 °C over 5 mm of liquid. Prusa measured layer adhesion more than doubled.[29] | Dichloromethane cement welds the resin, but the fibre keeps the joint from flowing closed. Controlled carcinogen.[30] |
Material entries describe families or representative grades, not an interchangeable specification for every spool. Test methods, orientations and conditions may differ. Unknown values are marked “Not documented”. Prices and source dates remain historical snapshots; check the linked guide for product details. Differences highlight text, not a universal winner.
Sources for this comparison
- Polymaker ABS Pro Technical Data Sheet V1 (2026-05-29) Polymaker · 2026-05 · tds
- Polymaker ABS Max Technical Data Sheet V1.1 (2026-06-01) Polymaker · 2026-06 · tds
- PolyLite ABS Technical Data Sheet (V5.5 served at this URL) Polymaker · 2024-11 · tds
- XSTRAND GF30-PC Data Sheet Owens Corning · 2019-04 · tds
- Polymaker product catalogue Polymaker · 2026-08 · vendor
- BASF Ultrafuse PC GF30 Black 2.85 mm 1.000 g igo3d · 2026-08 · vendor
- SUNLU E-ABS (Easy ABS) 3D Printer Filament 1 kg SUNLU · 2026-08 · vendor
- YXPOLYER ABS Enhanced product page YXPOLYER · 2026-08 · vendor
- 3DXTech product catalogue 3DXTech · 2026-08 · vendor
- ABS / ASA / PC Usage Guide Bambu Lab Wiki · 2026-08 · doc
- PolyLite PC Technical Data Sheet V5.4 Polymaker · 2024-11 · tds
- ABS — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- Max volumetric speed Prusa Knowledge Base · 2026-08 · doc
- ABS — material basics Polymaker Wiki · 2026-08 · doc
- Filament Material Guide Prusa Knowledge Base · 2026-08 · doc
- Composite materials filled with carbon, kevlar or glass Prusa Knowledge Base · 2026-08 · doc
- Polycarbonate — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- Wet Filament — signs, causes and drying Polymaker Wiki · 2026-08 · doc
- PC — material basics Polymaker Wiki · 2026-08 · doc
- TECANAT natural (PC) — stock shape properties Ensinger · 2026-08 · tds
- Experimental data for creep and dynamic mechanical properties of polycarbonate and polycarbonate/ABS Data in Brief 42:108264 · 2022-06 · paper
- Bambu Filament Technical Data Sheet V3.0 — ABS Bambu Lab · 2026-08 · tds
- Characterization of Thermal Expansion Coefficient of 3D Printing Polymeric Materials Using Fiber Bragg Grating Sensors Materials 17(18):4668 · 2024-09 · paper
- Emissions of Ultrafine Particles and Volatile Organic Compounds from Commercially Available Desktop Three-Dimensional Printers with Multiple Filaments (Azimi et al.) Environmental Science & Technology 50(3) 1260-1268 · 2016-01 · paper
- HIPS — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- Chemical resistance — resistance of Ensinger plastics to chemicals (DIN 50 014, 23/50) Ensinger · 2026-08 · tds
- Makrolon — The chemical resistance (Makrolon 2800, 6 days at 23 °C and 50 °C) Covestro · 2016-12 · tds
- HIPS — Knowledge Base Prusa Research · 2026-08 · doc
- Improve your 3D prints with chemical smoothing Prusa Research · 2026-08 · doc
- Weld-On 3 Acrylic Plastic Cement — technical data sheet (shipped as dichloromethane) IPS Corporation · 2002-07 · tds