Filament comparison
ABS-GF vs PETG-ESD
Compare printing settings, strength, heat resistance, dated prices and sources.
2 selected · all documented properties
| Property | Glass-fibre ABS (ABS-GF)ABS | ESD-safe PETGPETG |
|---|---|---|
| Market snapshot | ||
| Listing priceUSD/kg; dated snapshots | $34.99/kg median; $24.49–$73.33/kg across 4 dated product listings | $102.99/kg median; $65.98–$140.00/kg across 2 dated product listings |
| Identity & Market | ||
| Base polymer / chemistry | ABS reinforced with chopped glass fibre — 3DXTech's grade is nominally 10 wt%[1][2] | PETG compounded with a conductive filler to bring surface resistivity into the static-dissipative range[3][4] |
| Densityg/cm³ | 1.08 (Bambu Lab) and 1.15 (3DXTech), ISO 1183[2][1] | 1.24 (Fiberon) and 1.28 (3DXTech), ISO 1183[3][4] |
| Typical priceUSD/kg | 1 kg-equivalent spools span 24–73; the middle of the market is about 35[5][6][7][8] | 1 kg-equivalent spools span 66–140; the middle of the market is about 103[9][6] |
| Price range across brandsUSD/kg | 24–73 across brands; Siraya Tech 24, Bambu Lab 30, SUNLU 40, 3DXTech 73[5][6][7][8] | 66–140 across brands; Fiberon PETG-ESD 66, 3DXSTAT ESD-PETG 140[9][6] |
| Market availability1–5 | Available from several mainstream brands[5][6] | Niche, a handful of specialist brands[9][6] |
| Spool sizes & diameters | 1.75 and 2.85 mm; 750 g and 1 kg spools[6][5] | 1.75 mm; 0.5, 0.75, 1 and 3 kg spools[9][6] |
| Typical applications | Stiff, dimensionally stable enclosure and tooling parts; Bambu Lab notes the fibre blurs layer lines into a matte finish[2] | Electronics fixtures, trays and jigs handled around static-sensitive components[3][4] |
| Printing Parameters | ||
| Nozzle temperature°C | 240–280 (Bambu Lab)[2] | 250–290 (Fiberon)[3] |
| Bed temperature°C | 80–100 (Bambu Lab)[2] | 70–80 (Fiberon); 70 (3DXTech)[3][4] |
| Enclosure / chamber requirement1–5 | Enclosure recommended — Bambu Lab specifies a 45–60 °C chamber[2][10] | Open frame is fine — Fiberon specifies room-temperature chamber[3] |
| Recommended chamber temperature°C | 45–60 (Bambu Lab)[2] | Not documented |
| Part cooling fan | 0–80 % (Bambu Lab)[2] | Not documented |
| Bed surface & adhesion aid | Clean the plate and apply glue; Simplify3D also lists Kapton tape and ABS slurry[10][11] | Textured PEI, satin or powder-coated sheets; on smooth PEI a glue stick acts as a release agent[12][13] |
| Maximum volumetric flow (mm³/s; see test conditions)mm³/s | 14 at Bambu Lab's 180 mm/s cap on a 0.4 mm nozzle at 0.2 mm layer[2][14] | Fiberon rates the material to 500 mm/s, equivalent to 40 on a 0.4 mm nozzle at 0.2 mm layer — a machine-limited headline rather than a measured melt rate[3][14] |
| Warping tendency1–5 | Moderate — needs adhesion aid or draught shield; Bambu Lab positions the fibre as reducing warping[2] | Not documented |
| Bed-adhesion difficulty1–5 | Needs a specific surface plus adhesive[10] | Needs the right surface or a thin adhesive — the problem is releasing the part, not sticking it[12][13] |
| Stringing / oozing tendency1–5 | Slight — Polymaker advises 1–2 mm retraction at 20–30 mm/s[15] | Moderate — retraction tuning needed; Polymaker names stringing as PETG's common quirk[13] |
| Overall printing difficulty1–5 | Intermediate — dry filament and a tuned profile; hardened nozzle mandatory[10] | Intermediate — dry filament and a tuned profile; resistivity depends on getting the nozzle temperature right[3] |
| Hardware Wear & Reliability | ||
| Nozzle hardness required1–4 | Hardened steel required[10] | Hardened steel required[3] |
| Abrasiveness1–5 | Highly abrasive — standard GF composite[10] | Moderately abrasive — conductive carbon filler[3] |
| Nozzle clog risk1–5 | Moderate — needs dry filament and a clean nozzle; 3DXTech specifies a hardened 0.4 mm minimum nozzle and 0.25 mm layers or higher for the glass-filled grade[16][17] | Low — 3DXTech lists no special nozzle concerns and no minimum layer height for its ESD-PETG, only a 65 °C pre-dry[18] |
| Heat-creep / jam sensitivity1–5 | Slightly sensitive[11] | Slightly sensitive[19] |
| Hotend requirement | No special hot-end required[11] | No special hot-end required[19] |
| Moisture Behaviour | ||
| Moisture absorption (hygroscopicity)1–5 | Moderate — 0.53 % saturated at 25 °C / 55 % RH (Bambu Lab)[2] | Moderate (0.3–0.8 %) — the PETG matrix reaches 0.40 % saturated at 25 °C / 55 % RH and 3DXTech specifies a 65 °C, 4 h pre-dry[12][18] |
| Equilibrium moisture content at ~50 % RH% | 0.53 saturated at 25 °C / 55 % RH (Bambu Lab)[2] | 0.41 equilibrium water absorption (Fiberon PETG-ESD)[3] |
| Drying temperature & time | 80 °C for 8 h (Bambu Lab)[2] | 65 °C for 3 h (Fiberon)[3] |
| Symptoms when wet | Bubbling and popping at the nozzle, stringing and a rough surface[20] | Bubbling and popping at the nozzle, stringing and a rough surface[20] |
| Effect of moisture on strength | Polymaker rates ABS moderate-sensitivity and publishes no dry-versus-conditioned figures; absorbed water flashes to steam in the hotend and shows as bubbling and poor layer adhesion[20] | Polymaker groups PETG with nylon, PVA and TPU as highly hygroscopic; no dry-versus-conditioned strength figures are published for this grade and the loss shows as bubbling and poor layer adhesion[20] |
| Storage requirement | Sealed with desiccant; Polymaker rates ABS moderate-sensitivity[20] | Sealed with desiccant; Polymaker groups PETG with the highly hygroscopic materials[20][13] |
| Mechanical Properties | ||
| Tensile strength (XY)MPa | 36 ± 3 printed XY, ISO 527 (Bambu Lab); 3DXTech quotes 68 at break[2][1] | 36.1 ± 0.9 printed XY, ISO 527 (Fiberon); 3DXTech quotes 50 at break[3][4] |
| Young's modulusMPa | 3160 ± 170 printed XY, ISO 527 (Bambu Lab); 3DXTech quotes 4210[2][1] | 1983 ± 75 printed XY, ISO 527 (Fiberon)[3] |
| Elongation at break% | 6.3 ± 1.2 printed XY, ISO 527 (Bambu Lab); 3DXTech quotes 2 at break[2][1] | 7.3 ± 0.7 printed XY, ISO 527 (Fiberon); 3DXTech quotes 13 at break[3][4] |
| Flexural strengthMPa | 68 ± 4 printed XY, ISO 178 (Bambu Lab); 3DXTech quotes 70[2][1] | 54.0 ± 2.5 printed XY, ISO 178 (Fiberon)[3] |
| Flexural modulusMPa | 2860 ± 130 printed XY, ISO 178 (Bambu Lab); 3DXTech quotes 4420[2][1] | 1651 ± 141 printed XY, ISO 178 (Fiberon)[3] |
| Charpy impact, notchedkJ/m² | 4.2 ± 1.1 printed XY, ISO 179, notched (Bambu Lab)[2] | 5.7 ± 0.5 printed XY, ISO 179, notched (Fiberon)[3] |
| Other impact data | Charpy unnotched 14.5 ± 1.5 printed XY (Bambu Lab, ISO 179)[2] | Charpy unnotched 29.3 ± 2.2 printed XY (Fiberon, ISO 179)[3] |
| Layer adhesion / Z tensileMPa | 29 ± 3 printed Z, ISO 527 (Bambu Lab)[2] | 20.7 ± 0.6 printed Z, ISO 527 (Fiberon)[3] |
| Brittleness1–5 | Brittle — snaps with little warning; notched Charpy falls from 21.5 to 4.2 kJ/m² against unfilled Bambu Lab ABS[2][21] | Moderate[3] |
| Creep resistance / sustained load1–5 | Good — no creep test found; chopped glass fibre lifts modulus to 3160 MPa against 2200 for unfilled Bambu Lab ABS[2][21] | Below average — no ESD-grade creep test; unfilled PETG sagged from 12 to 17.1–20.4 mm over 5 days at 1.25 kg[22][23][24][25] |
| Fatigue / repeated-flex resistance1–5 | Below average — no S-N curve found; notched Charpy falls to 4.2 kJ/m² against 21.5 for unfilled Bambu Lab ABS[2][21] | Moderate — no ESD-grade S-N curve; unfilled printed PETG ran 79 000–193 000 cycles at 30 % of tensile strength[26] |
| Elasticity / flexibility1–5 | Rigid[2] | Slightly flexible in thin sections[3] |
| Z strength as % of XY% | 81 (Bambu Lab, printed Z against XY tensile)[2] | 57 (Fiberon, printed Z against XY tensile)[3] |
| Thermal Properties | ||
| HDT at 0.45 MPa°C | 99 (ISO 75, 0.45 MPa, Bambu Lab) against 87 for unfilled Bambu Lab ABS[2][21] | 76 (ISO 75, 0.45 MPa, Fiberon)[3] |
| HDT at 1.8 MPa°C | 88 (ISO 75, 1.8 MPa, Bambu Lab) against 84 for unfilled Bambu Lab ABS[2][21] | 72 (ISO 75, 1.8 MPa, Fiberon)[3] |
| Glass transition (Tg)°C | Not documented | 77 (Fiberon) and 80 (3DXTech), DSC[3][4] |
| Melting point / Vicat°C | Not documented | Amorphous — no melting point; Vicat 86 (Fiberon, ISO 306)[3] |
| Flammability / UL 94 | Not documented | Flammable; no UL 94 rating published for standard grades[27] |
| Environment & Chemical | ||
| Chemical resistance | Good against weak acids, weak alkalis, oils and grease; dissolved by acetone[28] | Withstands acids, alkalis, oils and UV exposure[13] |
| Food contact | Not food safe — Polymaker cites potential chemical leaching[15] | Not certified for food contact as filament[13] |
| Biodegradability / compostability | Not biodegradable[15] | Not biodegradable[13] |
| Recyclability | Mechanically recyclable but not accepted in household plastic collection[15] | Not accepted in household plastic collection[13] |
| Electrical & ESD properties | Not documented | Surface resistivity falls with nozzle temperature: 7.0×10⁶–1.6×10⁷ ohm at 250 °C, 3.2×10⁵–4.7×10⁵ at 270 °C and below 1×10⁴ at 290 °C (Fiberon); 3DXTech quotes 10⁷–10⁹ ohm/sq[3][4] |
| Health & Safety | ||
| Fume toxicity1–5 | High — hazardous VOC such as styrene; enclosure and filtration needed[29][10] | Moderate — measurable VOCs and UFPs, ventilation advised[29] |
| VOC emission rateµg/min | 12–113 styrene, the dominant VOC from every ABS and HIPS combination tested[29] | Not documented |
| Ultrafine-particle emission rateparticles/min | 2 × 10¹⁰ to 9 × 10¹⁰ median across all ABS printers, two orders of magnitude above PLA's ≈1 × 10⁸[29] | Not documented |
| Hazardous species emitted | Styrene dominates. Bambu Lab states ABS and ASA release harmful gases such as styrene at printing temperature, which can be toxic and cause dizziness or nausea[29][10] | Not documented |
| Ventilation / filtration requirement1–5 | Enclosure with carbon and HEPA filtration — an enclosure alone cut measured UFP by only about 35 %[29][10] | Open a window / occasional ventilation[29] |
| Dust & fibre handling hazard | Glass fibre is bound in the matrix; avoid inhaling sanding dust[1] | Conductive carbon filler is bound in the matrix; avoid inhaling sanding dust[3] |
| Post-Processing | ||
| Sanding & machining | Sands well and takes filler before painting[15] | Sands poorly — the material is tough and gums rather than powders[19] |
| Painting & finishing | Paints readily after light abrasion[15] | Not documented |
| Gluing & solvent welding | Not documented | Cyanoacrylate; no common solvent welds PETG cleanly[19] |
| Vapour / chemical smoothing | Not documented | No practical vapour smoothing[19] |
| Support material pairing | HIPS breaks away or dissolves in d-limonene; Bambu Lab sells a dedicated Support for ABS[30][10] | Prints its own supports; Polymaker rates PolyDissolve S1 for PETG[19] |
| Dimensional accuracy & detail | Bambu Lab describes a smooth matte finish with micro-spot gloss that blurs layer lines[2] | Nozzle temperature has to be held steady — it moves surface resistivity by three orders of magnitude[3] |
| Solvents & Solubility | ||
| Soluble in | Acetone dissolves the resin and leaves the fibre as sludge; MEK, THF, ethyl acetate and chlorinated solvents do the same.[31][28] | No common workshop solvent; 1,2-dichloroethane destroys it inside a week and dichloromethane — a carcinogen — dissolves the surface.[32][33] |
| Softened or crazed by | Petrol and perchloroethylene soften it and benzene attacks it; d-limonene disrupts layer adhesion in some ABS and ASA grades.[31][34] | Acetone (+16 % weight over 1 year at 23 °C), ethyl acetate, toluene and DMF swell and soften it; methanol crazes it.[32] |
| Solvent welding & smoothing agent | Acetone vapour reaches only the resin fraction, so the fibre is left standing proud of the smoothed surface.[33][28] | Dichloromethane brushed on is the only agent that smooths PETG — a controlled carcinogen, not workshop stock.[33] |
Material entries describe families or representative grades, not an interchangeable specification for every spool. Test methods, orientations and conditions may differ. Unknown values are marked “Not documented”. Prices and source dates remain historical snapshots; check the linked guide for product details. Differences highlight text, not a universal winner.
Sources for this comparison
- FibreX ABS+GF10 Glass Fiber ABS Technical Data Sheet 3DXTech · 2026-08 · tds
- Bambu Filament Technical Data Sheet V1.0 — ABS-GF Bambu Lab · 2026-08 · tds
- Fiberon PETG-ESD Technical Data Sheet V1.1 Polymaker · 2026-08 · tds
- 3DXSTAT ESD-PETG Technical Data Sheet 3DXTech · 2026-08 · tds
- ABS-GF — product page Bambu Lab US Store · 2026-08 · vendor
- 3DXTech product catalogue 3DXTech · 2026-08 · vendor
- Siraya Tech Fibreheart ABS-GF Filament product page Siraya Tech · 2026-08 · vendor
- SUNLU ABS-GF (ABS Glass Fiber) 3D Printer Filament 1 kg SUNLU · 2026-08 · vendor
- Polymaker product catalogue Polymaker · 2026-08 · vendor
- ABS / ASA / PC Usage Guide Bambu Lab Wiki · 2026-08 · doc
- ABS — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- Prusament PETG Technical Datasheet v1.1 Prusa Polymers · 2022-02 · tds
- PETG — material basics Polymaker Wiki · 2026-08 · doc
- Max volumetric speed Prusa Knowledge Base · 2026-08 · doc
- ABS — material basics Polymaker Wiki · 2026-08 · doc
- FIBREX ABS+GF — product page (print recommendations) 3DXTech · 2026-08 · doc
- Composite materials filled with carbon, kevlar or glass Prusa Knowledge Base · 2026-08 · doc
- 3DXSTAT ESD-PETG — product page (print recommendations) 3DXTech · 2026-08 · doc
- PET and PETG — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- Wet Filament — signs, causes and drying Polymaker Wiki · 2026-08 · doc
- Bambu Filament Technical Data Sheet V3.0 — ABS Bambu Lab · 2026-08 · tds
- PCTG vs PETG comparison — results spreadsheet My Tech Fun (Igor Gaspar) · 2026-08 · test
- Extrudr PETG vs PCTG vs XPETG-CF — results spreadsheet My Tech Fun (Igor Gaspar) · 2026-08 · test
- Prusament PETG-CF vs PETG V0 vs PETG — results spreadsheet My Tech Fun (Igor Gaspar) · 2026-08 · test
- BambuLab PETG Basic vs Translucent vs PETG-CF — results spreadsheet My Tech Fun (Igor Gaspar) · 2026-08 · test
- Mechanical Properties of Additively Manufactured Polymeric Materials — PLA and PETG — For Biomechanical Applications Polymers 16(13):1868 · 2024-06 · paper
- Prusament PETG V0 Technical Datasheet Prusa Polymers · 2026-08 · tds
- PolyLite ABS Technical Data Sheet (V5.5 served at this URL) Polymaker · 2024-11 · tds
- Emissions of Ultrafine Particles and Volatile Organic Compounds from Commercially Available Desktop Three-Dimensional Printers with Multiple Filaments (Azimi et al.) Environmental Science & Technology 50(3) 1260-1268 · 2016-01 · paper
- HIPS — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- Chemical resistance — resistance of Ensinger plastics to chemicals (DIN 50 014, 23/50) Ensinger · 2026-08 · tds
- Eastman Spectar copolyester — Chemical resistance (unstressed bars, 1 year at 23 °C) Eastman Chemical Company · 2026-08 · tds
- Improve your 3D prints with chemical smoothing Prusa Research · 2026-08 · doc
- HIPS — Knowledge Base Prusa Research · 2026-08 · doc