Filament comparison
PC-GF vs TPU 85A
Compare printing settings, strength, heat resistance, dated prices and sources.
2 selected · all documented properties
| Property | Glass-fibre PC (PC-GF)PC | TPU 85AFLEX |
|---|---|---|
| Market snapshot | ||
| Listing priceUSD/kg; dated snapshots | $71.27/kg median; $71.27–$71.27/kg across 1 dated product listings | $89.89/kg median; $31.99–$106.05/kg across 6 dated product listings |
| Identity & Market | ||
| Base polymer / chemistry | Polycarbonate reinforced with 30 wt% short glass fibre[1] | Soft thermoplastic polyurethane at 82–85 Shore A[2][3][4] |
| Densityg/cm³ | 1.17 (measured on a 100 % infill printed part, ISO 1183-A)[1] | 1.11 (BASF Ultrafuse 85A) to 1.19 (NinjaFlex 85A), ISO 1183 / ASTM D792[4][2] |
| Typical priceUSD/kg | 1 kg spools cluster near 71[5] | 1 kg-equivalent spools span 32–106; the middle of the market is about 90[6][7][2] |
| Price range across brandsUSD/kg | 71 — BASF Ultrafuse PC GF30 at igo3d is the only priced listing found; Owens Corning sells XSTRAND GF30-PC in 500 g and 1 kg[5][1] | 32–106 across brands; Siraya Tech Flex TPU 85A 32 at 1 kg, add:north TPU Pro Matte 85A 72, Recreus Filaflex 82A 90 at 500 g, Proto-pasta Clear Flexible TPU 90, 3DXTech 3DXFLEX 85A 96, NinjaTek NinjaFlex 106[8][6][7][9][2] |
| Market availability1–5 | Niche, a handful of specialist brands — neither Polymaker's nor 3DXTech's polycarbonate range contains a glass-fibre grade, but BASF Forward AM and Owens Corning both sell one through European retail[5][1][10][6] | Available from several mainstream brands[6][8] |
| Spool sizes & diameters | 1.75 and 2.85 mm at +/- 0.05 mm; 500 g and 1 kg net spools[1] | 1.75, 2.85 and 3 mm; 0.5, 1 and 2 kg spools[6][8][2] |
| Typical applications | Functional prototyping for mechanical engineering, electronics and automotive[1] | Soft-touch grips, seals, wearables and anything that must compress and rebound[2][3] |
| Diameter tolerance± mm | +/- 0.05 (Owens Corning XSTRAND)[1] | Not documented |
| Printing Parameters | ||
| Nozzle temperature°C | 280-330 (Owens Corning XSTRAND GF30-PC)[1] | 200–220 (BASF Ultrafuse 85A, 210 typical)[4] |
| Bed temperature°C | 80-110 (Owens Corning XSTRAND GF30-PC)[1] | 40 (BASF Ultrafuse 85A)[4] |
| Enclosure / chamber requirement1–5 | Enclosure required (passive) — as for unfilled PC[11][12] | Open frame is fine[4] |
| Bed surface & adhesion aid | Perforated plate, DimaFix or Magigoo PC glue (Owens Corning)[1] | PEI sheet or painter's tape; Polymaker warns TPU can over-stick and advises a glue stick as a release agent[13][14] |
| Maximum volumetric flow (mm³/s; see test conditions)mm³/s | Not documented | 1.2–3.2 at the 15–40 mm/s BASF specifies on a 0.4 mm nozzle at 0.2 mm layer[4] |
| Warping tendency1–5 | Not documented | None[4] |
| Bed-adhesion difficulty1–5 | Not documented | Sticks to anything — Recreus states its 82A grade has excellent bed adhesion without a heated bed or additives[3] |
| Stringing / oozing tendency1–5 | Not documented | High — drying plus tuning needed[15][14] |
| Overall printing difficulty1–5 | Not documented | Advanced — enclosure, hardware upgrades, tuning; at this hardness the filament will not push through a Bowden tube[2][3] |
| Extruder requirement | Owens Corning specifies a nozzle above 0.4 mm and hardened steel nozzles and drive wheels[1] | Direct drive only. NinjaTek calls its 85A grade ideal for direct-drive extruders and Recreus specifies direct-drive printers for 82A; BASF caps print speed at 15–40 mm/s with a nozzle of 0.4 mm or larger[2][3][4] |
| Hardware Wear & Reliability | ||
| Nozzle hardness required1–4 | Hardened steel required — Owens Corning states glass reinforcement shortens brass nozzle and drive-wheel life[1] | Brass fine indefinitely[16] |
| Abrasiveness1–5 | Highly abrasive — 30 wt% glass fibre[1] | Non-abrasive[16] |
| Nozzle clog risk1–5 | High — jams from moisture, heat creep or particles; PC already absorbs water from the air and Prusa lists glass-filled composites as a higher clogging risk[17][18] | High — jams from moisture, heat creep or particles[15][14] |
| Heat-creep / jam sensitivity1–5 | Not documented | Very high — softens in the cold zone readily; soft filament buckles between the drive gear and the melt zone[14][2] |
| Hotend requirement | Not documented | No special hot-end required, but a direct-drive extruder is (Simplify3D)[13] |
| Moisture Behaviour | ||
| Moisture absorption (hygroscopicity)1–5 | Negligible (<0.1 % EMC) — Owens Corning measures below 0.1 % at 23 °C and 50 % RH (ISO 62)[1] | Moderate — NinjaTek measures 0.22 % in 24 h (ASTM D570) and BASF specifies a 70 °C dry for at least 5 h[2][4] |
| Equilibrium moisture content at ~50 % RH% | Below 0.1 at 23 °C and 50 % RH, and below 0.1 at saturation (ISO 62)[1] | 0.22 after 24 h water immersion (NinjaFlex 85A, ASTM D570) — an immersion figure, not an equilibrium moisture content at 50 % RH[2] |
| Drying temperature & time | Not documented | 70 °C for at least 5 h in a hot-air dryer or vacuum oven (BASF)[4] |
| Symptoms when wet | Not documented | Bubbling and popping at the nozzle, stringing and a rough surface[15] |
| Effect of moisture on strength | No dry-versus-conditioned figures are published. Polymaker calls PC highly hygroscopic; absorbed water flashes to steam and shows as bubbling and poor layer adhesion[19][15] | Polymaker groups TPU with the highly hygroscopic materials; wet TPU prints with poor layer adhesion and weak, brittle layers[15] |
| Storage requirement | Not documented | Sealed with desiccant; often kept in a dryer during the print[15] |
| Mechanical Properties | ||
| Tensile strength (XY)MPa | 65 at break (printed, ISO 527 at 1 mm/min)[1] | 26 ultimate (NinjaFlex 85A, ASTM D638)[2] |
| Young's modulusMPa | 5400 (printed, ISO 527 at 1 mm/min)[1] | 12 (NinjaFlex 85A, ASTM D638) — two orders of magnitude below any rigid filament; NinjaTek's 95A Cheetah reaches 26 by the same method[2][20] |
| Elongation at break% | 2.5 at break (printed, ISO 527 at 1 mm/min)[1] | 650 at break (Filaflex 82A) and 660 (NinjaFlex 85A); BASF measures 600 in XY and 320 in ZX[3][2][4] |
| Flexural strengthMPa | 113 at yield (printed, ISO 178 at 2 mm/min)[1] | Not documented |
| Flexural modulusMPa | 5500 (printed, ISO 178 at 2 mm/min)[1] | Not documented |
| Brittleness1–5 | Brittle — snaps with little warning; 2.5 % elongation at break[1] | Very ductile — bends far before failing[2] |
| Hardness (scale-specific)Shore A / Shore D / Rockwell | Rockwell 70 (118) — the source does not name the scales and Shore D 79 on extruded unfilled PC stock (ASTM D785, D2240); no figure is published for a glass-fibre grade[21] | 29 Shore D / 85 Shore A (BASF Ultrafuse 85A, ISO 7619-1); 85 Shore A (NinjaFlex, ASTM D2240); 82 A nominal for Filaflex[2][4][3] |
| Creep resistance / sustained load1–5 | Excellent — holds load for years. Room-temperature tensile creep of moulded unfilled PC ran unbroken at 41 MPa until the test was stopped, and 30 wt% glass raises the tensile modulus from about 2.3 to 5.4 GPa[22][1] | Poor — no 85A creep test; a printed 95A TPU bar crept from 74.5 to 82.7 mm over 5 days at 1.25 kg, and softer grades creep more[23] |
| Fatigue / repeated-flex resistance1–5 | Not documented | Excellent — living hinges viable[14] |
| Elasticity / flexibility1–5 | Rigid[1] | Rubbery / highly elastic[2][3] |
| Z strength as % of XY% | Not documented | 53 — BASF measures 320 % elongation at break in ZX against 600 % in XY[4] |
| Wear resistance & friction | Not documented | Abrasion 0.08 g mass loss over 10 000 cycles (NinjaFlex, ASTM D4060); 82 mm³ (BASF, ISO 4649)[2][4] |
| Thermal Properties | ||
| HDT at 1.8 MPa°C | 137 (printed, ISO 75 Method A at 1.8 MPa)[1] | Not documented |
| Glass transition (Tg)°C | 145 (DSC, ISO 11357)[1] | Not documented |
| Melting point / Vicat°C | 270 stated as melting point (ISO 11357) — unusual for an amorphous polymer, but this is the published figure[1] | 216 melting (NinjaFlex 85A, DSC)[2] |
| Thermal expansion (CTE)µm/m·K | 26.2 in XY and 77.4 in Z (printed, ISO 11359-2) — a threefold anisotropy, and the lowest in-plane expansion of any polycarbonate here[1] | Not documented |
| Flammability / UL 94 | UL 94 V-0 verified (Owens Corning)[1] | Not documented |
| Environment & Chemical | ||
| UV resistance1–5 | Good — years with some colour shift. Owens Corning lists UV resistance as a product benefit but publishes no exposure data[1] | Good — years with some colour shift; Polymaker lists UV exposure among the conditions TPU withstands[14] |
| Chemical resistance | Not documented | Withstands industrial solvents and UV exposure (Polymaker)[14] |
| Water / humidity resistance in service1–5 | Excellent — essentially unaffected; below 0.1 % water at saturation (ISO 62)[1] | Not documented |
| Food contact | Not documented | Not food safe without specific certification (Polymaker)[14] |
| Biodegradability / compostability | Not documented | Not biodegradable[14] |
| Recyclability | Not documented | Not accepted in household plastic collection[14] |
| Electrical & ESD properties | Electrically insulating (Owens Corning)[1] | Not documented |
| Health & Safety | ||
| Fume toxicity1–5 | Moderate — measurable VOCs and UFPs, ventilation advised[24] | Low hazard — minimal VOC and particle emission; TPU was not among the nine filaments in the chamber study[24] |
| Ultrafine-particle emission rateparticles/min | ≈4 × 10¹⁰ median — the highest ultrafine-particle rate of the nine filaments in the chamber study, above every ABS tested[24] | Not documented |
| Ventilation / filtration requirement1–5 | Ventilated room or enclosure recommended[24][12] | Open a window / occasional ventilation[24] |
| Dust & fibre handling hazard | Owens Corning warns that the glass reinforcement is abrasive when melted and advises sufficient ventilation and avoiding extrusion fumes[1] | Not documented |
| Post-Processing | ||
| Sanding & machining | Not documented | Difficult to sand or smooth; Polymaker limits post-processing to trimming or tumbling[14] |
| Gluing & solvent welding | Not documented | Cyanoacrylate bonds TPU; no common solvent welds it[14] |
| Vapour / chemical smoothing | Not documented | No practical vapour smoothing[14] |
| Support material pairing | Not documented | Polymaker warns TPU supports are often very difficult to remove[14] |
| Dimensional accuracy & detail | High dimensional stability is the headline benefit; the 26.2 um/m*K in-plane CTE is a third of unfilled PC's[1] | Not documented |
| Solvents & Solubility | ||
| Soluble in | Dichloromethane and chloroform dissolve the matrix and leave the fibre; DMF and dioxane do the same (Covestro).[25] | DMF, DMSO, NMP and THF dissolve TPU; acetone, MEK and cyclohexanone are partial solvents. All laboratory reagents.[26] |
| Softened or crazed by | Methanol, butyl acetate, ether, 1 % NaOH and phthalate plasticisers stress-crack it; acetone, MEK and xylene swell it.[25] | Toluene and benzene swell it up to +50 % by weight at 23 °C; esters swell it severely; ethanol and IPA soften it.[26] |
| Solvent welding & smoothing agent | Dichloromethane cement welds the resin, but the fibre keeps the joint from flowing closed. Controlled carcinogen.[27] | None practical — the true solvents (DMF, THF, NMP) are laboratory reagents and leave the joint swollen and weak.[26] |
Material entries describe families or representative grades, not an interchangeable specification for every spool. Test methods, orientations and conditions may differ. Unknown values are marked “Not documented”. Prices and source dates remain historical snapshots; check the linked guide for product details. Differences highlight text, not a universal winner.
Sources for this comparison
- XSTRAND GF30-PC Data Sheet Owens Corning · 2019-04 · tds
- NinjaFlex 85A Technical Specifications NinjaTek · 2026-08 · tds
- Filaflex 82A product page (Shore hardness and elongation) Recreus · 2026-08 · vendor
- Ultrafuse TPU 85A Technical Data Sheet (Version 3.0) BASF Forward AM · 2022-08 · tds
- BASF Ultrafuse PC GF30 Black 2.85 mm 1.000 g igo3d · 2026-08 · vendor
- 3DXTech product catalogue 3DXTech · 2026-08 · vendor
- Siraya Tech Flex TPU 85A Filament — product page Siraya Tech · 2026-08 · vendor
- Proto-pasta product catalogue Proto-pasta · 2026-08 · vendor
- add:north TPU Pro Matte 85A product page add:north · 2026-08 · vendor
- Polymaker product catalogue Polymaker · 2026-08 · vendor
- PolyLite PC Technical Data Sheet V5.4 Polymaker · 2024-11 · tds
- ABS / ASA / PC Usage Guide Bambu Lab Wiki · 2026-08 · doc
- Flexible (TPE/TPU) — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- TPU — material basics Polymaker Wiki · 2026-08 · doc
- Wet Filament — signs, causes and drying Polymaker Wiki · 2026-08 · doc
- Extrudr Product Catalogue (DURAPRO PA12 data block) Extrudr · 2025-03 · tds
- Composite materials filled with carbon, kevlar or glass Prusa Knowledge Base · 2026-08 · doc
- Polycarbonate — Ultimate 3D Printing Materials Guide Simplify3D · 2026-08 · doc
- PC — material basics Polymaker Wiki · 2026-08 · doc
- NinjaTek technical specs comparison chart (Cheetah, NinjaFlex, Armadillo, Alloy 910, Nylon 645) NinjaTek · 2026-08 · tds
- TECANAT natural (PC) — stock shape properties Ensinger · 2026-08 · tds
- Experimental data for creep and dynamic mechanical properties of polycarbonate and polycarbonate/ABS Data in Brief 42:108264 · 2022-06 · paper
- BambuLab TPU 95A HF vs Qidi TPU 95A HF — results spreadsheet My Tech Fun (Igor Gaspar) · 2024-02 · test
- Emissions of Ultrafine Particles and Volatile Organic Compounds from Commercially Available Desktop Three-Dimensional Printers with Multiple Filaments (Azimi et al.) Environmental Science & Technology 50(3) 1260-1268 · 2016-01 · paper
- Makrolon — The chemical resistance (Makrolon 2800, 6 days at 23 °C and 50 °C) Covestro · 2016-12 · tds
- Elastollan — Chemical properties: swelling and chemical resistance BASF · 2026-08 · tds
- Weld-On 3 Acrylic Plastic Cement — technical data sheet (shipped as dichloromethane) IPS Corporation · 2002-07 · tds